Without having seen the images, it is almost certain that you are seeing
dendrites. These are caused by the presence of ionic contamination under
the mask. If it is hygroscopic, you will absorb sufficient humidity to
cause this.
The most usual cause (but not unique) is insufficient cleaning of the
boards before the mask is applied. The prehistoric MIL-P-55110x standard
specified pre-masking ionic cleanliness levels for this very reason.
You can download a short video showing real time dendrite formation at
http://www.bnellis.com/dendrites/
Brian
- Bogert wrote:
> September 8, 2004
>
> A technical challenge for all you printed wiring board (PWB) manufacturing experts. Please help.
>
> The attached photographs show conductive contamination trapped under LPI solder mask covered over by Type UR conformal coating (.003 in nominal thickness).
>
> The PWB is a two sided PTH (no SMT parts) board of FR-4 (thickness range is .062 to 0.125 inch depending on the PWB part number) with solder mask applied over bare copper. The PWB is used in a military application. The PTH are tin-lead. The same type contamination has also been found on multi-layer PWB'S.
>
> The photos show what look like tin whiskers (I do not think they are since SEM analysis shows the material as a combination of tin, lead and copper and normally tin whiskers grow only on virgin plating such as pure tin, silver, zinc, etc.).
>
> I have two questions as follows and request your expert opinions in answering the questions:
>
> 1) What process or material problem could have caused the conductive filaments to form, and how to prevent it from happening again? My best guess is contamination residue from the etch-back process.
>
> 2) If the PWB passes shorts testing and end-item functional test, is there any concern with continued use in a humid environment given that the contamination is trapped under a layer of solder mask as well as a layer of Type UR conformal coating.
>
> Any info available on how long solder mask and conformal coating can retard moisture entry? I know that neither material will prevent eventual moisture entry. Is there any data that shows how long these materials will retard moisture from causing dendrite growth problems?
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
> -----------------------------------------------------
> Any concern for dendrite growth or other no-no's?
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|