TECHNET Archives

August 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Rodney Miller <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Rodney Miller <[log in to unmask]>
Date:
Thu, 3 Aug 2006 10:08:30 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (93 lines)
So Anchoring barrel wall is not recommended on higher Tg/Td laminate
systems due to Cu CTE...

Could I get a copy of that White paper?  I'm interested in the cause
effect also...

We have seen similare problems arise from trace/pad interface and
fracturing.  If what you say is good for Barrel, this may also have
limits that are being exceeded.  Our conventional wisdom is to teardrop
or filet the interface from Annular ring to Trace, to help with the
migration of a mechanical fracture.

Will this logic still apply?

LoHst and Confused...

-----Original Message-----
From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: Wednesday, August 02, 2006 5:23 PM
Subject: Re: Barrel to Laminate Adhesion loss


Hi Richard & All,
Actually, the higher occurrances of hole wall separation and trace
separation
are not so much caused by more lateral stresses, but the different
thermal
and mechanical properties of SAC solders.
To understand what is happening, one really needs to understand what the

whole damage process causing hole wall separation [sometimes also called
resin
recession] and inner-layer separation [also called post separation or
trace
separation.
(1) On heating the resin expands-because of the glass fiber
reinforcement it
is prevented to expand in x/y and thus expands in z at nearly 3-times
its
thermal expansion without the glass reinforcement]; there is an
exception to this- the resin also tries to expand into the volume
occupied by the PTH, and is of
course, to some degree at least, prevented from doing so by the Cu
barrel
plating.
Thin Cu plating and/or large separation between inner-layer land
[serving as
anchors] encourage larger bulging inwards of the Cu with plastic
deformation
of the Cu.
(2) On cooling, the resin contracts to its former volume-if the Cu is
plastically deformed to a significant degree, it cannot do so: the
result=>hole wall
separation, and near the surface in connection with land rotation
inner-layer
separation.
(3) For SnPb solders the Solidus is 183C; thus, Solidus - Tg
(183-170C)~13C. For SAC solders the solidus is 217C; thus, Solidus - Tg
(217-170C)~47C. The consequence is that the delta-T after solder
solidification is about
4-times larger for SAC-solders, over which the high above Tg-thermal
contraction
acts-and this also holds the Cu back to its former position: the result
=>more
hole wall separation, and inner-layer separation.

Pretty straight-forward when you think about.

Werner

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2