Someone asked about the material composition:
The pins are tin plated and the socket contacts are gold plated.
There is no evidence of corrosion or galvanic action here.
A laboratory used a SEM to determine the presence of carbon and FTIR to rule
out the presence of any significant quantities of carbon containing
compounds--none was detected.
Another common sense point: electrical arcing between two metal conductors
with the production of a "carbon appearing" deposit at the point where the
arcing occurs is a phenomenon with which most people are familiar.
I would like to understand the process better--including the source of the
carbon.
Searching through physics, chemistry, electronics, failure analysis and
other literature has failed to give me a clue.
If someone has a clue as to where I can find some relevant literature on
this subject I am very interested in hearing from you.
Thanks again.
> -----Original Message-----
> From: TechNet [SMTP:[log in to unmask]] On Behalf Of Dehoyos, Ramon
> Sent: Friday, March 26, 2004 7:59 AM
> To: [log in to unmask]
> Subject: Re: [TN] Carbon Buildup On Tin Plated Contacts
>
> That is very true most of the sockets are reliable. If there is
> any defect such as the fingers of the sockets not putting enough pressure
> on the inserted pin or the fingers not properly secured ( loose,
> fingers of the sockets are inserted into the socket housing ) or fingers
> fall down and collapsed when a pin is inserted, then there will be arcing
> and carbon build up.
> Regards,
> Ramon
>
> > -----Original Message-----
> > From: Crepeau, Phil (Space Technology)
> > Sent: Thursday, March 25, 2004 8:16 PM
> > To: [log in to unmask]
> > Subject: Re: [TN] Carbon Buildup On Tin Plated Contacts
> >
> > hi,
> >
> > i know what you all are talking about. nevertheless i just want to say
> that many mil spec digital, power, and rf mil spec connectors have gold
> pins and sockets and they are extremely reliable.
> >
> > phil
> >
> > -----Original Message-----
> > From: David Douthit [mailto:[log in to unmask]]
> > Sent: Thursday, March 25, 2004 4:35 PM
> > To: [log in to unmask]
> > Subject: Re: [TN] Carbon Buildup On Tin Plated Contacts
> >
> >
> > Bogert,
> >
> > Based on this, we are prohibiting use of sockets for new design
> equipment. Most military equipment prohibits use of sockets (ref
> historical MIL-STD-2000). In my opinion, no equipment that is intended
> for long term reliability should ever use sockets.
> >
> > I agree. Even gold to gold contacts can become intermittent due to
> deposition of
> > particles and reactive gases combined with micro vibration and or
> thermal excursions.
> >
> > David A. Douthit
> > Manager
> > LoCan LLC
> >
> >
> >
> > - Bogert wrote:
> >
> > >What is the material finish of the socket contacts? Is it the same as
> the part pins? If not, you could have corrosion issue due to different
> finishes. For example tin plated pins inserted into socket with gold
> plated contacts could be problem. Another problem could be spread socket
> contacts that cause poor electrical connections resulting in arcing and
> subsequent carbon deposits. Unfortunately we have used numerous sockets
> in fielded equipment with significant quality issues. Based on this, we
> are prohibiting use of sockets for new design equipment. Most military
> equipment prohibits use of sockets (ref historical MIL-STD-2000). In my
> opinion, no equipment that is intended for long term reliability should
> ever use sockets.
> > > ----- Original Message -----
> > > From: Chafin, Ken G.<mailto:[log in to unmask]> To:
> [log in to unmask]<mailto:[log in to unmask]> Sent: Wednesday, March 24, 2004
> 5:10 PM
> > > Subject: [TN] Carbon Buildup On Tin Plated Contacts
> > >
> > >
> > > Elemental carbon has been identified as the dark material that has
> > > "developed" on the surface of a pin at the point where it makes
> electrical
> > > contact with a socket.
> > >
> > > The applied voltage in one case is 12 VDC and in another it is 5 VDC.
> > >
> > > It is suspected that the high vibration environment in which the
> device
> > > operates is causing intermittent opening of the contact area and
> electrical
> > > arcing is causing the carbon deposition.
> > >
> > > I believe I have seen literature which identifies atmospheric C0_2 as
> the
> > > primary source of the carbon (possibly some CO also).
> > >
> > > Can anyone refer me to literature which confirms, disconfirms or
> otherwise
> > > provides enlightenment on the precise nature of this process?
> > >
> > > Thanks
> > >
> > > ---------------------------------------------------
> > > Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> > > To unsubscribe, send a message to
> [log in to unmask]<mailto:[log in to unmask]> with following text in
> > > the BODY (NOT the subject field): SIGNOFF Technet
> > > To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
> > > To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
> > > Search the archives of previous posts at:
> http://listserv.ipc.org/archives<http://listserv.ipc.org/archives>>
> > > Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/conten
> tpage.asp?Pageid=4.3.16> for additional information, or contact Keach
> Sasamori at [log in to unmask]<mailto:[log in to unmask]> or 847-509-9700 ext.5315
> > > -----------------------------------------------------
> > >
> > >---------------------------------------------------
> > >Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> > >To unsubscribe, send a message to [log in to unmask] with following text
> in
> > >the BODY (NOT the subject field): SIGNOFF Technet
> > >To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > >To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> > >Search the archives of previous posts at:
> http://listserv.ipc.org/archives
> > >Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> > >-----------------------------------------------------
> > >
> > >
> > >
> > >
> >
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> > To unsubscribe, send a message to [log in to unmask] with following text
> in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at:
> http://listserv.ipc.org/archives
> > Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> > -----------------------------------------------------
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> > To unsubscribe, send a message to [log in to unmask] with following text
> in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at:
> http://listserv.ipc.org/archives
> > Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> > -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|