John
IMHO there is no such thing as good solder in dross. You will find that metal recovered
thus will always have large quantities of oxides in suspension and these will form
nuclei for further dross formation. If you put it back in the pot, the rate of dross
formation will increase. This is why the initial fill and topping-up of the pot should
be with dross-reduced solder and why, even when metallic impurities are within limits,
the solder should be regularly changed (when dross formation becomes excessive).
Brian
parrrrr rossss wrote:
> Hi,
>
> I have a question about dorss recycling :
>
> Is there any off-line equipment in market
> to separate the good solder from the dross ( waste
> collected from the wave solder pot) ?
>
> John
>
> __________________________________________________
> Do You Yahoo!?
> Talk to your friends online with Yahoo! Messenger.
> http://im.yahoo.com
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> information.
> If you need assistance - contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> ##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|