TECHNET Archives

January 2011

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Mike Fenner <[log in to unmask]>
Reply To:
Date:
Fri, 14 Jan 2011 11:07:45 +0000
Content-Type:
text/plain
Parts/Attachments:
text/plain (244 lines)
Some corrosion, once started, can self perpetuate by feeding on atmosphere
water and CO2, with no need for differential metals etc.

Regards
 
 
Mike

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Eric Christison
Sent: Friday, January 14, 2011 10:48 AM
To: [log in to unmask]
Subject: Re: [TN] a different Friday quiz

I'd go for galvanic corrosion in a mildly corrosive atmosphere, or 
possibly highly corrosive depending upon your taste in food.

You didn't ever drop it in a bowl of Kimchi did you, or that Icelandic 
dish of basking shark marinated in caustic soda?

Imagine periods of high humidity and temperature changes where moist 
contaminated (salty?) air is drawn into the enclosure where it condenses 
on the screw head. I bet you have dissimilar metals connected together 
which will cause corrosion and the condensing air will drip off the 
screw head to move the corrosion products around the inside of the device.

Regards,







On 14/01/2011 09:39, Steven Creswick wrote:
> Inge,
>
> I feel your pain.  I had purchased a more expensive unit - supposedly
having
> a significant range from transmitter to receiver.  Was going to place the
> transmitter by my windsock.  Wrong!  First Summer it became erratic.  All
> manner of flux residues and funky things growing inside the transmitter.
> Don't know what flux was used, but they certainly used plenty of it.  Was
> difficult to clean, but doing so has resolved all the problems except for
> range.
>
> I have to go way further West to get to the board assembler.  Two words
come
> to mind - cheap, chinchy.  Pretty mediocre quality.
>
> In my case, I did not get the value I expected to have paid for
>
> Could the screw plating [under the head] have been poor?  ... add flux
> residues and humidity during shipment, and as Robert said - a wire
beneath?
>
>
> Steve Creswick
> http://www.linkedin.com/in/stevencreswick
>
>
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Robert Kondner
> Sent: Thursday, January 13, 2011 7:01 PM
> To: [log in to unmask]
> Subject: Re: [TN] a different Friday quiz
>
> Inge,
>
>   I will take a wild guess, there is copper under the screw somewhere,
right?
>
> Bob K.
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge
> Sent: Thursday, January 13, 2011 6:07 PM
> To: [log in to unmask]
> Subject: [TN] a different Friday quiz
>
> I bought a digital temperature equipment, consisting of a inhouse table
unit
> and a outdoors unit. Cost = 25 USD. Cheap? Yes. But let's have a look on
> inside after the problem, which started just a few weeks. You can read the
> inside temperature, clock works, date works, and you can use the alarm and
> shift between the four channels, but the receiver does not take in the
> signals from the little sender on the  wall any more. I dismantled the box
> and marvelled when I saw the shit I payed for. It's a wonder that there
are
> any functions working at all! Now, what caused the dead receiver was a
flow
> of iron from one screw (upper left  corner ) . There is a bridge of
> corrosion products  (brown and green) from the screw to the thermistor
(RT)
> continuing to the rest of the circuitry.  When I washed the card and dried
> it, the reciever worked again,
>
> Now, folks, here comes a question for the sharp TNetters:
>
> "How can the screw be so rusty and deliver iron ions when it's not
connected
> to anything? It's just torqued into the plastic body. The other screws are
> identical, but  have not been involved in anything. "
>
> The box has been on the kitchen table and has not been exposed to humidity
> or any else abnormal condition.
>
> The two 1.5 V batteries are removed on the pics.
>
> Hope the gregorian Steve will help me with the photos.
>
> /Inge
>
>
>
>
>
>
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in the
> BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
> (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet
> NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
> e-mail to [log in to unmask]: SET Technet Digest Search the archives of
> previous posts at: http://listserv.ipc.org/archives Please visit IPC web
> site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for
additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
> ext.2815
> -----------------------------------------------------
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site
> http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
> ext.2815
> -----------------------------------------------------
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site
http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
> -----------------------------------------------------
> .
>

-- 
Eric Christison
Consumer&  Micro group
Imaging Division

STMicroelectronics (R&D) Ltd
33 Pinkhill
Edinburgh EH12 7BF
United Kingdom

Tel:	+44 (0)131 336 6165
Fax:	+ 44 (0)131 336 6001

The contents of the email are ST confidential.




______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------


***This email, its content, and any files transmitted with it, are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient, please contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination, or other use of, or taking of any action in reliance upon this information by persons or entities other than the intended recipient is prohibited.

Messages sent via this medium may be subjected to delays, non-delivery, and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.***


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2