Reducing the solder temperature to only slightly hotter than what is needed for good solder joint formation, and perhaps switching to SN100C will help reduce the pin dissolution, and thus allow a longer dwell time along the areas where there is a change of direction without any ill effects.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Peter Wong
Sent: Wednesday, July 09, 2014 10:15 AM
To: [log in to unmask]
Subject: Re: [TN] Dissolving pins
Good morning,
After looking at our program, I've discovered that there are 4 locations along the length of this connector where we are actually dwelling for 4 seconds and moving along at 3 mm/sec. The dissolved pins seem to follow the pattern of where we stop and dwell for those 4 seconds.
Thanks to everyone for the suggestions. I think we need to preheat the boards in a different manner versus how we are doing it now.
Thanks again for your insights.
Peter
-----Original Message-----
From: Peter Wong
Sent: Tuesday, July 08, 2014 2:35 PM
To: [log in to unmask]; 'Wayne Thayer'
Subject: RE: Dissolving pins
Thanks everyone,
It's been so long for me that I forgot about SAC305 eroding metals. I will get our tech to pull up the program to get more details about dwell times and nozzle speeds.
I believe our temperature is set that high to assist with solder fill. What solder pot temperatures are others running for SAC305?
Peter
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Wayne Thayer
Sent: Tuesday, July 08, 2014 1:51 PM
To: [log in to unmask]
Subject: Re: [TN] Dissolving pins
Hi Peter-
SAC305 is well known for eroding metals. 325C sounds pretty darned hot to me! Why so high?
I have run a solder fountain rework station filled with SAC305, and it was very difficult to stop it from eroding the ends of the via barrels. That was only at 230C!
Wayne Thayer
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Peter Wong
Sent: Tuesday, July 08, 2014 4:32 PM
To: [log in to unmask]
Subject: [TN] Dissolving pins
Hi Everyone,
We ran some assemblies where after selective soldering with SAC305, the phosphor bronze leads on a Harwin connector look to have been dissolved.
The solder pot temperature is set at 325 deg C and we dwelled on each pin for no more than 3 seconds. We are using an OA flux. Harwin tells me that the melting point of the pins is 954 deg C.
We are having the solder in our selective solder pot analyzed to see if there is anything out of spec that could be causing this.
Has anyone else experienced something similar or does anyone have an idea as to what could be causing this?
A photo is available at the following link.
http://ipc-technet.groupsite.com/galleries/show/27385
Thanks
Peter
________________________________
The enclosed documents are proprietary items to Silicon Forest Electronics'
(SFE) customers. They shall not be reproduced nor disclosed for any purpose except as specified in writing from an authorized agent of SFE. These documents may contain data restricted for export by the International Traffic in Arms Regulations (ITAR) section of the Arms Export Control Act (or the Export Administration Act). Violators are subject to severe criminal penalties.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|