Frank
We just made some PCB's with some lead free alloys ( SnAgCu, SnAg, SnZn, Castin) and our industrial partner that did the tests had to admit that all solder joints satisfied their internal quality standards. Also to me, the solder joints did look good according to IPC-A-610. The interesting thing was, that the boards where soldered with a standard profile, where only the peak was set on 233°C ( 12°C above liquidus for SnAg !). The results so far indicate
- The flux chemistry has a bigger influence on wetting than the alloy
- The joints are not so much dull than, well I don't know whether I get the right English term, rippled. These ripples are a result from the internal structure of the joint and I even believe IPC-A-610 might not need to be changed for lead free solder.
Guenter Grossmann
Swiss Federal Institute for Materials Testing and Research EMPA
Centre for Reliability
8600 Duebendorf
Switzerland
Phone: xx41 1 823 4279
Fax : xx41 1823 4054
mail: [log in to unmask]
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|