The only way to remove solder from gold (assuming it is fully wetted) is to
strip all the underlying gold off the finger and replate. The solder will have
dissolved much of the gold (if not all) under the joint, forcing replating of
the finger anyway.
There are commercial strippers and plating solutions available (I saw some adds
a few years ago) that can strip and replate that one finger and avoid scrapping
the panel..
______________________________ Reply Separator _________________________________
Subject: Gold Finger Touch Up
Author: Denis Meloche <[log in to unmask]> at INTERNET
Date: 6/16/97 1:50 PM
Does anyone have information on how to repair gold edge connectors which
have solder on them? I remember a product or service from the late 70's or
early 80's which purported to fix this. Can anyone shed some light on the
subject? I have seen the defect repaired by reflowing with Au80/Sn20 but I
am unsure of the long term reliability of this method.
Thanks,
Denis Meloche
Heraeus Inc
610-825-6050
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************