I have seen the voids you describe caused by wet holes at the
image pre-clean process. Moisture in the holes softens the
dry film resist over the hole and the vacuum from panel cooling
draws it into the hole. The developer leaves a perfect ring of
resist in the hole just down from the knee.
-----Original Message-----
From: Julie Dixon [mailto:[log in to unmask]]
Sent: Tuesday, December 14, 1999 8:42 AM
To: [log in to unmask]
Subject: [TN] Ring Voids
Dear TechNet,
What would cause a perfect ring void just under the knee of the hole, with
the knee
intact? Drill, DML, Dry film, light scrub, Pre plate clean- acid cleaner &
Na
Persulfate Etch 10-15 micro inches, Acid CU, Acid bright Tin, Mono DF strip,
Ammoniacal
Etch. Job specific to 1 part # all other product running along side is
perfect.
All material Std. .062 Fr-4 1/1. Longtime runner w/ no probs in past.
Thanks,
Julie Dixon
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|