There are no 'specifications for the X-Ray inspection.' There are also no
specifications as to ball shape. From a quality point of view the only thing that
counts is a good metallurgical bond. However, from a reliability point of
view, the more non-uniform [squashed down] the solder balls are the earlier they
will fail under identical conditions—this is primarily caused by the reduced
solder ball height, and to a lesser extent the non-uniform geometry.
Elongated soldering pads have been shown to give slightly more cycles to
failure than circular ones.
Werner
**************************************
Get a sneak peek of the all-new AOL at
http://discover.aol.com/memed/aolcom30tour
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------