I've seen what I think is a similar problem. I'll describe it and how I
cured it and see if it will help you.
Problem: 50% of surface pads wetted on ENIG surfaces at customer location.
Research: LPI coated panels were ENIG plated. Found peeling LPI and panels
were stripped in an alkaline solution and then LPI reapplied. Suspected that
the alkaline stripping solution or the LPI developer solution (potassium
carbonate ?) had somehow remained on the immersion gold surface.
Cure: After panels are recoated with LPI they must be processed in a hot
alkaline cleaner(cleaner on our black oxide process)then rinsed well and
100% wetting was restored.
Theory: Alkaline contamination was not rinsed from either the stripper or
the developer and ruined the gold surface for solderability. On the chemical
principal that likes-dissolve-likes the hot alkaline cleaner removed this
contaminant and with proper rinsing no residueS remained.
I hope this is helpful.
Russ Burdick
>From: Heinz Mader <[log in to unmask]>
>Reply-To: "TechNet E-Mail Forum." <[log in to unmask]>
>To: [log in to unmask]
>Subject: [TN] Adhesion problems of galvanic gold on electroless nickel gold
>Date: Wed, 28 Nov 2001 09:32:36 -0600
>
>Hallo outthere in the big pcb world
>A qestion from switzerland
>We produce a board(material G 10) After full plating electroless nickel
>gold the adhesion is good.Then we laminate fotoresist film for goldmask and
>develope with soda.
>We let plate the bond gold externel. This Gold has not enough adhesion
>with tape test We see that not later not after Galvanic plating
>
>Has anyone some experince solving that problem
>
>
>With kind regards
>
>Heinz Mader
>Ascom AG
>3000 Berne
>Switzerland
>
>---------------------------------------------------------------------------------
>Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt delivery of Technet send the following message: SET
>Technet NOMAIL
>Search previous postings at: www.ipc.org > On-Line Resources & Databases >
>E-mail Archives
>Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
>additional
>information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
>ext.5315
>---------------------------------------------------------------------------------
_________________________________________________________________
Get your FREE download of MSN Explorer at http://explorer.msn.com/intl.asp
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|