TECHNET Archives

February 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Fri, 12 Feb 2010 07:30:49 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
Douglas Pauls <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="ISO-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (168 lines)
There Dave goes, typing before he has had his diet Coke.

Soldering:  everyone knows this is the act of setting your drywall on fire 
with a blowtorch as you attempt to fix that slow leak in the copper pipe.

Brazing:  what you do with a really fine rack of ribs on the grill

Welding - a small dent on the wall of your well.

Somedays that man takes an awful lot of shepherding.......

Doug Pauls



"David D. Hillman" <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
02/12/2010 07:19 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]


To
[log in to unmask]
cc

Subject
Re: [TN] Old reference for silver solder - what's it cross ref to?






Hi Steve - you are correct, there are three basic definitions have been 
established to keep soldering, brazing and welding from becoming confused 
terms:

Soldering - the joining of two metals by heating them to a suitable 
temperature below their solidus and applying a filler metal having a 
liquidus temperature below 450C

Brazing - the joining of two metals by heating them to a suitable 
temperature below their solidus and applying a filler metal having a 
liquidus temperature above 450C

Welding - the joining of two metals by heat or pressure, with or without a 

filler metal, to produce a localized union through fusion 

Sometimes folks use brazing and soldering interchangeably.

Dave



Steven Creswick <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
02/11/2010 07:06 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Steven Creswick <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] Old reference for silver solder - what's it cross ref to?






Graham,

I thought I would have an earlier version as well, but alas I do not.

In any case, my recollection was that this spec was for the more generic
'solders' [at <300-400°C liquidus] and not the more higher temp 'brazes'
like the 780°C CuAg eutectic. 

My use of the terms 'solders' and 'brazes' may not be totally correct 
[Dave
H can provide clarification], but I would suggest, as others have, that 
the
'silver' solder you are looking for is the low temp Sn62 Pb36 Ag2 [Sn62 at
180°C], or Sn96.3 Ag 3.7 [which we used to call 'Sn96/4' or Sn96 at 
221°C],
both being eutectic solders.

We used to use both for soldering on thick film Ag, Pd/Ag, or Pt/Pd/Ag's 
to
mitigate leaching of the Ag bearing inks.

Since this is apparently for a PWB application, I think one could 
reasonably
argue that anything above Sn96/4 is unlikely to be desired.

Get snow?!  Michigan dug out again.  Will let you know how the next round
is..

Steve C





______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 

for additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2