I've witnessed sporadic poor covered pads but never even considered
verifying their connection via traces to the varied pads.
Typical cause in the majority I observed were poor tin strip/poor predip
(75% of observed) and poor resist develop (15% of observed) with the
remaining undetermined.
Of the observations made above, these were in instances where we confirmed
bath operating optimally.
Is there enough (electrical) activity occurring in these baths where a short
or other board condition would result in robbing plating from those type
areas???
Franklin
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dennis Fritz
Sent: Monday, September 18, 2006 7:03 PM
To: [log in to unmask]
Subject: Re: [TN] ENIG
In a message dated 9/18/2006 7:50:57 P.M. Eastern Daylight Time,
[log in to unmask] writes:
There is one thing I did leave out. The pads that aren't taking ENIG all
happen to be in the same net. Has anyone encountered this?
To me, this says that there is some "electrical" cause, stronger than the
catalyst that initiates the electroless nickel plating. Remember, the
catalyst in the ENIG process is a tightrope between getting plating
everywhere (extraneous plating) and not covering some pads (skip plating).
Here you have skip plating
If the same net skips board-to-board, likely it is a design issue where
something is grounded out unintentionally and plating is getting defeated
in one spot. It could be that some via is tented consistantly holding a
poisoning fluid - tin stripper for instance. If different nets skip on the
panel, then I suspect a more random error - incomplete tin strip, etc. I
guess it could
be marginally weak catalyst. I would expect developer residues to be
random
pads - not all in a single net. Something "electrical" is going on here.
Denny Fritz
MacDermid
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|