TECHNET Archives

November 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Michelle Masaitis <[log in to unmask]>
Date:
Thu, 18 Nov 2010 09:40:26 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Robert DeQuattro <[log in to unmask]>
Subject:
From:
Robert DeQuattro <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="iso-2022-jp"
MIME-Version:
1.0
Parts/Attachments:
text/plain (78 lines)
It could be a problem related to the component MSL and proper handling.  Many led's are MSL 4 which gives these components only a 72 hour floor life outside of their special moisture barrier bag packaging before special handling (normally baking) is required.  The first step is to find out the component MSL.  Then you can refer to J-std-033B for details on how to handle.



Bob DeQuattro
Quality Manager
VR Industries, Inc
333 Strawberry Field Road, STE 6
Warwick, RI 02886
Tel: 401-732-6800 ext 45
Fax: 401-738-7910
[log in to unmask]
www.vrindustries.com



------------------------------------------------------------------------------------------------------------------------
This email message is for the sole use of the intended recipient(s) and may contain confidential and privileged information. Any unauthorized use or disclosure is prohibited. If you are not the intended recipient, please contact the sender by reply email and destroy all copies of the original message.



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Michelle Masaitis
Sent: Thursday, November 18, 2010 8:42 AM
To: [log in to unmask]
Subject: [TN] Led Failures Please help

-   the through-hole LED in question is made by company "EOI ", and their 
part number is  "EOZ-ZARNCD0-DG " (s 
-   according to the component spec sheet  (enclosed), the maximum 
temperature for the component is 260℃ 
-   the maximum temp and wave contact time we initially used is  249℃ , 4-6 
seconds.  We saw some defects after first pass, usually about .2%, but one 
month as high as 1.5%.   After successful testing, there were then some 
latent defects that occurred at our customer or their end customer.  The 
defects are erratic, sometimes the LEDs work, and sometimes they don't 
-  the supplier recommended a lower temperature and shorter exposure profile 
so we used SAC305 solder with maximum temp of 244.4℃ and 3 seconds.  
There 
were no defects after first pass and testing, but again we had some latent 
defects occur at customer 
-   for reference, we run many similar LED from other manufacturers 
(OSRAM&Lumiled, also spec at 260℃) at temperatures of 251℃ and 4-7 
seconds 
and see no such problems. 

Attached is a wave profile.

Please let me know if you seen a similar issue and what caused it.


Thanks

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2