Thanks everyone for all great ideas...the problem found is mainly IC
coplanarity.
Solder did not wick up on 1 to 2 of 66 TSOP lead bends but when cross
sectioned the IC coplanarity measured was within IC MFR's spec. The
solder paste height was measured within spec too prior reflow.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Guy Ramsey
Sent: Thursday, February 14, 2008 8:30 AM
To: [log in to unmask]
Subject: Re: [TN] Minimum Heel Fillet Height
Essentially, it says the solder fillet needs to be 50% of the thickness
of
the heel bend or lead thickness (depending on the package). The "G"
thickness is there to prevent someone from saying, "It would have been
50%
of the lead thickness, if the lead were coplanar".
None of these are intended to be measured. They are visual criteria. In
my
opinion, if companies out there using measuring tools trying prove
acceptance are miss using the standard.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Herminia Guevarra
Sent: Wednesday, February 13, 2008 6:01 PM
To: [log in to unmask]
Subject: [TN] Minimum Heel Fillet Height
Hi, folks,
Can anybody please explain in details how the minimum heel fillet height
criteria for Class 2 was computed and specified?
F= solder thickness (G) + 50% lead thickness
Can solder thickness be solder paste height prior reflow?
What about if leads are not coplanar? What would be the spec for co
planarity? How can they be measured?
Need reply...
Thanks,
Herminia
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
14/2/2008NOT INTENDED AS A SUBSTITUTE FOR A WRITING
NOTHING IN THIS E-MAIL, IN ANY E-MAIL THREAD OF WHICH IT MAY BE A PART, OR IN ANY ATTACHMENTS THERETO, SHALL CONSTITUTE A BINDING CONTRACT, OR ANY CONTRACTUAL OBLIGATION BY PNY, OR ANY INTENT TO ENTER INTO ANY BINDING OBLIGATIONS, NOTWITHSTANDING ANY ENACTMENT OF THE UNIFORM ELECTRONIC TRANSACTIONS ACT, THE FEDERAL E-SIGN ACT, OR ANY OTHER STATE OR FEDERAL LAW OF SIMILAR SUBSTANCE OR EFFECT. THIS EMAIL MESSAGE, ITS CONTENTS AND ATTACHMENTS ARE NOT INTENDED TO REPRESENT AN OFFER OR ACCEPTANCE OF AN OFFER TO ENTER INTO A CONTRACT. NOTHING IN THIS E-MAIL, IN ANY E-MAIL THREAD OF WHICH IT MAY BE A PART, OR IN ANY ATTACHMENTS THERETO SHALL ALTER THIS DISCLAIMER.
This e-mail message from PNY Technologies, Inc. is for the sole use of the intended recipient(s) and may contain confidential and privileged information. Any unauthorized review, use, disclosure or distribution is prohibited. If you are not the intended recipient, please contact the sender by reply e-mail and destroy all copies of the original message.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|