TECHNET Archives

July 2009

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Neil Maloney <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Neil Maloney <[log in to unmask]>
Date:
Tue, 14 Jul 2009 11:28:16 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (283 lines)
Ditto for the early Chrysler Sebring/ Dodge Stratus instrument panel. A
pair of PTH power resistors on the backside of the instrument cluster
PWB would heat cycle, vibrate and open up at the solder joints. This
would intermittantly make the odometer go blank and shut off the tach. A
lot of clusters were swapped out because of it. Only 30 sec. with a
soldering pencil would solve the problem. 

Neil Maloney, Manufacturing Engineer/
LAN Administrator
Contemporary Control Systems, Inc
2431 Curtiss St Downers Grove, IL  60515
(630) 963-7070 x132
[log in to unmask]
http://www.ccontrols.com
http://www.ctrlink.com
 


   

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge
Sent: Tuesday, July 14, 2009 11:15 AM
To: [log in to unmask]
Subject: Re: [TN] NTC (It's not Friday, but this is so true!)


Wayne,
this was a classical High Current/High Temperature/Solder 
Decomposition/Fatigue issue. (Is there one word for this?). Famous
failure, 
world wide during a couple of years with Philips Z12 TV chassis many
years 
ago. Philips decided to solder mount the image frequency transformer by 
means of a number of pins in through holes on the PWB. The transformer
was 
very warm, heavy and lots of current passed through the pins. The 
transformer had no screws or bolts, was just hanging in the solder
joints. 
After some time, the solder joints looked EXACTLY like the one in my AC 
controller board. Those who were familiar with the technology at that
time 
knew what to do: open the TV swing out the monster chassis, suck up the
old 
solder around the transformer pins and redo the soldering. This had to
be 
repeated once a year or so. Philips made a redesign and fixed a
mechanical 
suppor which removed all mechanical force to the solder joints. All old
dogs 
recognize this kind of issue, younger don't .

AND....this type of failures exist still. The below lines are written
just a 
few years ago:

TV and Monitor Manufacturing Quality and Cold Solder Joints
Low cost no-name (or unknown name) computer monitors tend to be
particularly 
prone to bad solder connections. However, so are many models of name
brand 
TVs including those from RCA/GE/Proscan and Sony. We'll touch on these
at 
the end of this article.
Any intermittent problems with monitors that cause random sudden changes
in 
the picture brightness, color, size, or position are often a result of
bad 
connections. Strategically placed bad connections can also cause parts
to 
blow. For example, a bad connection to the SCR anode in a phase
controlled 
power supply can result in all the current passing through the startup 
resistor, blowing it as well as other components. I had a TV like this -
the 
real problem was a bad solder joint at a pin on the flyback. Thus,
erratic 
problems, especially where they are power or deflection related, should
not 
be ignored!

Bad solder joints are very common in TVs and monitors due both to poor 
quality manufacturing as well as to deterioration of the solder bond
after 
numerous thermal cycles and components running at high temperature.
Without 
knowing anything about the circuitry, it is usually possible to cure
these 
problems by locating all bad solder connections and cleaning and
reseating 
internal connectors. The term 'cold solder joint' strictly refers to a 
solder connection that was either not heated enough during
manufacturing, 
was cooled too quickly, or where part pins were moved before the solder
had 
a chance to solidify. A similar situation can develop over time with
thermal 
cycling where parts are not properly fastened and are essentially being
held 
in by the solder alone. Both situations are most common with the pins of

large components like transformers, power transistors and power
resistors, 
and large connectors. The pins of the components have a large thermal
mass 
and may not get hot enough during manufacturing. Also, they are
relatively 
massive and may flex the connection due to vibration or thermal
expansion 
and contraction.

Why Can't TV Manufacturers Learn to Solder Properly?
I can think of several potential reasons - all solvable but at higher 
manufacturing cost.
  1.. Mass of large component leads (like shields) does not get
adequately 
heated during manufacture leading to latent cold solder joints. While
they 
may look OK, the solder never actually 'wetted' the heavy pins and
therefore 
did not form a good mechanical or electrical bond.

  2.. Thermal cycles and differential thermal coefficients of circuit 
boards, traces, and solder. While it is not easy to do anything about
the 
material properties, using plated through-holes or a similar mechanical
via 
would greatly increase the surface area of the joint and prevent the 
formation of cracks.

  3.. Vibration. This is also directly related to the single sided
circuit 
boards without plated through-holes to strengthen the joints.

  4.. Lack of adequate mechanical support (single sided circuit boards 
without plated through-holes (vias).
I believe that the single most significantimprovement would come about
by 
using plated through-holes but this would add to the cost and apparently
the 
consumer is not willing to pay more for better quality and reliability!
Some 
designs have used rivlets - mechanical vias instead of plated ones.
While 
this is good in principle, the execution has often been flawed where
cold 
solder joints resulted between the rivlets and the circuit board traces
due 
to lack of adequate process control.
The Sony and RCA/GE tuner shield problem is interesting because this
could 
have been solved years ago at essentially no additional cost as other 
manufacturers - and their own repair procedures - have proven.

The End


Inge

----- Original Message ----- 
From: "Thayer, Wayne - IIW" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, July 14, 2009 4:02 PM
Subject: Re: [TN] NTC (It's not Friday, but this is so true!)


Hi Inge!

I am also someone who takes stuff to pieces.  You should see the scars
on my 
knuckles from all of the sheet metal cuts you can get on a car.

Now that you've put your car back together....

Are you absolutely sure the solder joint was bad when it left the line?
I 
mean, the rest of the joints look just fine, so what is it about that
one? 
In all liklihood this was wave soldered.

What if the real problem is that too much current is going through that 
joint, which is considerably smaller than the adjacent joint on the same

trace?  You may have only peeled back the first layer of the onion!

I hate to put doubts in the mind of someone who did an excellent job
getting 
the thing repaired, but I know you are tough!

Wayne

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steven Creswick
Sent: Tuesday, July 14, 2009 3:55 AM
To: [log in to unmask]
Subject: Re: [TN] NTC (It's not Friday, but this is so true!)

Inge - wow!  It's all in the hunt!  Good find!

Steve - You are right!  That is a cool trailer!

Steve C




http://stevezeva.homestead.com/files/Inge_s_Car_Fun_.pdf



http://stevezeva.homestead.com/files/Unusual_Trike.jpg

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To 
unsubscribe, send a message to [log in to unmask] with following text in
the 
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or 
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet 
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send 
e-mail to [log in to unmask]: SET Technet Digest Search the archives of 
previous posts at: http://listserv.ipc.org/archives Please visit IPC web

site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional 
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100

ext.2815
-----------------------------------------------------

This e-mail and any files transmitted with it may be proprietary and are

intended solely for the use of the individual or entity to whom they are

addressed. If you have received this e-mail in error please notify the 
sender.
Please note that any views or opinions presented in this e-mail are
solely 
those of the author and do not necessarily represent those of ITT 
Corporation. The recipient should check this e-mail and any attachments
for 
the presence of viruses. ITT accepts no liability for any damage caused
by 
any virus transmitted by this e-mail.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask]
or 
847-615-7100 ext.2815
----------------------------------------------------- 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2