TECHNET Archives

August 2009

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Frank Kriesch <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Tue, 25 Aug 2009 15:49:05 +0200
Content-Type:
text/plain
Parts/Attachments:
text/plain (218 lines)
Ingemar,

Ipc-A-610 asks for clear appearance in all 3 classes. Bubbles aspecially 
between electrical connections are always an issue, because they reduce 
isolationresistance, are or might become a home for residues.

Regards

Frank





Hernefjord Ingemar <[log in to unmask]> 
Gesendet von: TechNet <[log in to unmask]>
25.08.2009 14:56
Bitte antworten an
TechNet E-Mail Forum <[log in to unmask]>; Bitte antworten an
Hernefjord Ingemar <[log in to unmask]>


An
[log in to unmask]
Kopie

Thema
Re: [TN] Antwort: Re: [TN] Manual spraying, further qs






Frank,
thanks for a hand. Think we have most of the IPC stds, so it ought to be 
somewhere in the paper mountain. 
Vital question: do all of you demand that the conformal coating shall be 
glass clear, and if so, why? 
/Inge

 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Frank Kriesch
Sent: tisdag 25 augusti 2009 11:20
To: [log in to unmask]
Subject: [TN] Antwort: Re: [TN] Manual spraying, further qs

Ingemar,

IPC-CC-830,Qualification and Preformance of Electrical Insulating Compound 
for PWB  tells you e.g. about the required apperance of Conformal Coating.
IPC-SM-840C, Table 1 lists all the requirements for the qualification of 
soldermasks. Adhesion Conformal Coating is one of them. But has to be 
agreed with user and supplier. 

Regards,

Frank






Inge <[log in to unmask]>
Gesendet von: TechNet <[log in to unmask]>
24.08.2009 23:38
Bitte antworten an
TechNet E-Mail Forum <[log in to unmask]>; Bitte antworten an Inge 
<[log in to unmask]>


An
[log in to unmask]
Kopie

Thema
Re: [TN] Manual spraying, further qs






Thanks Ken,
are there any stds that demand a perfect surface, e.g. any IPC standards. 
And what use to cause outgassing issues? I have several PWB courses 
behind, 
but many, many years ago. Can dig in my piles, but a faster answer from TN 


seems a bit more comfortable.
/Inge


----- Original Message ----- 
From: "Ken Bloomquist" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Monday, August 24, 2009 11:20 PM
Subject: Re: [TN] Manual spraying, further qs


> The bad board had beans for lunch, "bad out gassing problem"! :-)
>
> KennyB
>
> -----Original Message-----
> From: Inge [mailto:[log in to unmask]]
> Sent: Monday, August 24, 2009 1:50 PM
> To: [log in to unmask]
> Subject: Re: [TN] Manual spraying, further qs
>
> This very day, I couldn't stay aside but had to do something to help the
> production guys. So, I took a fresh, naked and qualified board from 
> another
> source and did this:
> Put one of our problem boards beside the reference board, both on bottom 


> of
> a larg well box, i.e. no fans blowing, nor any evacuation. Sprayed both
> simultaneosly. Inspected them after one hour at room  temp. The 
reference
> board was absolutely perfect, while the other was matte! Had a look in a
> microscope. The bad guy had thousands of microscopic inclusions and even
> superficial voids, the reference was perfect. Noticed that the bad 
boards
> have a much coarser (looks like the net pattern after screen 
> printing)green
> sheet (solder mask) and numerous voids already before spraying. What is 
> your
>
> opinion?
> /Inge
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text 
in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: 
http://listserv.ipc.org/archives
> Please visit IPC web site 
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
> for additional information, or contact Keach Sasamori at [log in to unmask] 
or 
> 847-615-7100 ext.2815
> ----------------------------------------------------- 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 

for additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815
-----------------------------------------------------



.
Der Inhalt dieser E-Mail ist für den Absender rechtlich nicht verbindlich.
Informieren Sie uns bitte, wenn Sie diese E-Mail fälschlicherweise 
erhalten haben (Fax: +49-7551-891-4001). Bitte löschen Sie in diesem Fall 
die Nachricht. Jede Form der weiteren Benutzung ist untersagt.
.
The content of this e-mail is not legally binding upon the sender.
If this e-mail was transmitted to you by error, then please inform us 
accordingly (Fax: +49-7551-891-4001). In such case you are requested to 
erase the message. Any use of such e-mail message is strictly prohibited.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------



.
Der Inhalt dieser E-Mail ist für den Absender rechtlich nicht verbindlich.
Informieren Sie uns bitte, wenn Sie diese E-Mail fälschlicherweise erhalten haben (Fax: +49-7551-891-4001). Bitte löschen Sie in diesem Fall die Nachricht. Jede Form der weiteren Benutzung ist untersagt.
.
The content of this e-mail is not legally binding upon the sender.
If this e-mail was transmitted to you by error, then please inform us accordingly (Fax: +49-7551-891-4001). In such case you are requested to erase the message. Any use of such e-mail message is strictly prohibited.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2