TECHNET Archives

June 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Mon, 13 Jun 2005 11:01:24 -0700
Reply-To:
Subject:
From:
Jana Carraway <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (63 lines)
Werner,

If it's black pad on the component side, how would Kerry prove or disprove
it?  Could he find the cause by using Auger or cross-section?  What would be
the appropriate tests to perform to find root cause?  Should he send a
component back to the supplier for root cause analysis?

Thank you,
Jana Carraway

Jana Carraway
MSEI - Advanced Technology Group
6024 S.W. Jean Road
Lake Oswego, OR  97035
503.697.5291, ext 1180
email: [log in to unmask]

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Werner Engelmaier
Sent: Monday, June 13, 2005 10:04 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2


Hi Kerry,
You most likely have 'Black Pad' on the componet side. That, together with
the stess concentration from the SMD-geometry, caused a briitle ionterfacial
overstress failure.

Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2