TECHNET Archives

March 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
[log in to unmask], TechNet E-Mail Forum <[log in to unmask]>
Date:
Wed, 1 Mar 2006 07:38:38 -0300
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Marcello Brett Malteze <[log in to unmask]>
Subject:
From:
Marcello Brett Malteze <[log in to unmask]>
X-cc:
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (135 lines)
We can see this voids on solder past after assembly process and I di not
know this Solectron papers?Would you send to me?
 
Tks a lot,
 
Marcello Brett

  _____  

From: [log in to unmask] [mailto:[log in to unmask]] 
Sent: sexta-feira, 24 de fevereiro de 2006 18:26
To: TechNet E-Mail Forum; Marcello Brett Malteze
Cc: [log in to unmask]
Subject: Re: [TN] Via in Pad x Voids on Solder Process



Marcello, 
Is this voids in the solder paste after assembly or voids in the board for
the sequential laminations?  Have you seen the Solectron paper on HDI VIP
voids as a function of blind-via placement and final finish? 
Happy Holden
Asian Pacific Materials 



Marcello Brett Malteze <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]> 


02/24/2006 03:40 PM 


Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Marcello Brett Malteze <[log in to unmask]>



To
[log in to unmask] 

cc

Subject
[TN] Via in Pad x Voids on Solder Process

	




Hey Team,





   We are facing some problems regarding voids on Via in Pad on a 10 layers

board with sequential lamination ( 3 times inside press) on BGA area ,

someone can give me light or share your experience on this?



Board Spec:



Dielectric 2 x 106 = 90 - 100 µm final

YAG machine

O/L Copper 12 µm

Laser Diameter 130 µm

Surface finish Immersion Tin



Sometimes Voids are so big that are creating shorts under BGA.



Marcello Brett Malteze 

Mechanical Process Engineering 

Mobile: + 55 11 9468 4833 

Skype: mbrett73 





Legal Disclaimer:

The information contained in this message may be privileged and
confidential. It is intended to be read only by the individual or entity to
whom it is addressed or by their designee. If the reader of this message is
not the intended recipient, you are on notice that any distribution of this
message, in any form, is strictly prohibited. If you have received this
message in error, please immediately notify the sender and delete or destroy
any copy of this message


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------



---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2