TECHNET Archives

August 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Bev Christian <[log in to unmask]>
Date:
Mon, 24 Aug 2009 07:36:13 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
Douglas Pauls <[log in to unmask]>
In-Reply-To:
<5A3CBC0AD3774E3BBCB0F123AC33AFBF@bev1a0f3c0a9bc>
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (470 lines)
Ahem, yes.  Although, if some manly soaps can have pumice, or crushed lava 
rock, perhaps a manly lotion can have crushed granite. 
Nahhhhhhhhh................

Doug Pauls



Bev Christian <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
08/21/2009 09:15 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Bev Christian <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] Contamination by Hand Sanitizers & Lotions






Doug,
I think you meant to write "pomegranate", not "pomegranite", unless this 
is
really some manly man stuff made out of crushed rock.
Bev 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Douglas Pauls
Sent: Friday, August 21, 2009 3:07 PM
To: [log in to unmask]
Subject: Re: [TN] Contamination by Hand Sanitizers & Lotions

Ohhhhh, alright.

So, my young co-op student, Mike, and I are putting together the 
evaluation plan.  We included the Techspray material because we have this 
already in house and Hillman qualified it about 10 years ago.  The Jergens 

hand lotion is fairly popular in this area and has some aloe vera in it. 
We wanted a non-aloe-vera hand lotion - a real "girly girl" lotion that 
would have the heavier scents and oils in them that might possibly 
transfer to the electronics.  One of the comments we have received off an 
on through the years is that the operators don't like the smell of the 
Techspray material.  And it is not so much a case of not liking the smell 
as preferring a lotion with a nicer fragrance.

So, I task Mike with finding a suitable Girly Girl kind of lotion.  Mike 
heads down to one of our local Bath and Body Works stores.  Now, Mike, 
like me, is a masculine, manly sort of man, and we take to such stores 
like a fish takes to the Sahara Desert.  The objective is to dash in, pick 

something quick, dash out.  Mike goes over the the older sales lady and 
describes what he is looking for.  The sales lady is actually a retired 
industrial engineer from one of the chemical processing companies here in 
Cedar Rapids.  So they start talking about the Design of Experiments 
(DOE), sample sizes, methods of measurement, etc.  Not really the kind of 
conversation you would expect to hear in your local Bath and Body works. 
So they wanted to pick a "worst case", a lotion that would stay with you 
for a while and maintained the fragrances for quite a time.  Exactly.  So, 

they settled on the Midnight Pomegranite, Mike bought a bottle, and then 
dashed out.

Now, I must say it has a very pleasant fragrence.  You open up the bottle 
and you smell it.  Even Dead-Nose Hillman could smell this stuff.  Put 
some on your hands and you will still smell it 3-4 hours later.

Doug Pauls



Randall L Bock <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
08/21/2009 01:24 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Randall L Bock <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] Contamination by Hand Sanitizers & Lotions






Your gona leave us hanging on the Bath and Body Works Midnight Pomegranite 

 !!!


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Douglas Pauls
Sent: Friday, August 21, 2009 2:18 PM
To: [log in to unmask]
Subject: Re: [TN] Contamination by Hand Sanitizers & Lotions

Well, I can briefly discussed what we have done so far.  These are the 
materials we have been looking at:

Purell hand sanitizer
Sams Club hand sanitizer
Germ-X Gnarley Green hand sanitizer (just because I want to use Gnarley in 


a technical report)
Jergen's Hand Lotion
Bath and Body Works Midnight Pomegranite (funny background story as to 
why)
Techspray's lotion (our current approved standard)

We have done a chemical analysis on the materials. 
Did an ionic transfer study using ceramic plates.  Nothing much transfers 
on the sanitizers, and no measurable ionics on lotions.
Did some SIR work - still have to analyze the data but at first glance 
nothing leaps out at me
Presently (today) doing solderability impacts
Dielectric Withstanding Voltage tests pending
Effects on adhesive bonding pending

Based on what I have seen so far, I don't really have too much of a 
concern on the hand sanitizers.  The vast majority evaporates, not much, 
if any gets transferred to the assembly, and we clean in house anyway 
prior to conformal coating.  The jury is still out on the hand lotions. If 


you are a no-clean house, you might have more of a concern than I have.

Chemically, if you forced me to pick one, go with the Purell.  The Sams 
Club stuff is cheaper, but has some noticable residues and the Purell 
seems cleaner. 

Remember, free advice is worth everything you pay for it, but I think you 
are OK if they are allowed in house.  Last summer, when Cedar Rapids went 
through its major flooding, we were asked to curtail water usage as much 
as possible to save the one remaining city well that had not flooded.  We 
used primarily hand sanitizers for 3-4 weeks rather than soap and water 
and we had no incidences during that time of contamination we could trace 
to these materials.

Doug Pauls



Roger Mack <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
08/21/2009 11:20 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]


To
[log in to unmask]
cc

Subject
Re: [TN] Contamination by Hand Sanitizers & Lotions






If there is any chance of getting results sooner I would be interested. 
Based on the earlier technet conversations we have not been supplying 
operators with sanitizers and encouraging hand washing. However, just like 



ESD lotion, whether you supply the floor or not, you have to be on the 
watch for unapproved materials from home being used.

Just this week the request for sanitizers has come up again with back to 
school and flue season only 2 weeks away. The recent flues going around do 



cause some panic and it would be great to have some data to back up any 
position we take on sanitizer use.


Roger Mack  P.Eng. 
Manufacturing Specialist
Parker Hannifin Corporation
Electronic Controls Division
1305 Clarence Avenue
Winnipeg, MB  R3T 1T4 Canada 
direct 204 453 3339 x373
www.vansco.ca
www.parker.com







Douglas Pauls <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
2009-08-21 10:45
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]


To
[log in to unmask]
cc

Subject
Re: [TN] Contamination by Hand Sanitizers & Lotions






Good morning all,

Being blessed with an abundance of bright young co-op students, we are 
doing a study of the topic here at Rockwell Collins.  The study will 
finish in a few weeks and I plan on publishing the results, probably at 
Apex.

Doug Pauls
Rockwell Collins



Brian Ellis <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
08/21/2009 01:17 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Brian Ellis <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] Contamination by Hand Sanitizers & Lotions






Apart from the thread on this subject here a month or two back, the only 
mention in literature that I know of is in my book, which discusses in a 
diagrammatic form not only the effect of lotions before and after 
soldering. Sanitisers didn't exist in those days, but their effect is 
similar to lotions, although their oily components are lower.

As an addendum to my post in the earlier thread, I was back in hospital 
for another operation last week and found that they had placed 
squirt-bottles of sanitisers every 5 m along all the corridors, 
presumably as an anti-H1N1 measure. This allowed me to have better 
access to the stuff and I found that the hand was persistently 
contaminated. I was able to repeat my mirror test 2 or 3 hours after 
deliberately using the sanitiser correctly, being careful not to handle 
anything in the meanwhile. As one of the components is a high molecular 
weight polymerised glycol, it is a reasonable assumption that this is 
the persistent substance. As it is hygroscopic, it is also a reasonable 
assumption that it's not going to improve sensitive electronics if 
transferred from the hand to an assembly. If such transfer occurs before 
soldering, then the heat may cause further polymerisation, rendering the 
hygroscopic residues more difficult, maybe impossible, to remove.

Brian

Diljit Matharu wrote:
> Can someone direct me to resources which talk about PCBAs contamination 
by the use of hand sanitizers & lotions.
> 
> 
> 
> Thanks,
> 
> 
> 
> Diljit S. Matharu
> Quality Leader - B C
> Creation Technologies
> 
> Office: 604.430.4336 x 3395 | Mobile: 778.240.8144
> 8977 Fraserton Court | Burnaby, BC, Canada | V5J 5G1
> [log in to unmask]<mailto:[log in to unmask]> 
| www.creationtech.com<http://www.creationtech.com/>
> 
> [cid:[log in to unmask]]Working together to build the future
> 
> 
> 
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text 
in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: 
http://listserv.ipc.org/archives
> Please visit IPC web site 
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional 
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 
ext.2815
> -----------------------------------------------------
> 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 




for additional information, or contact Keach Sasamori at [log in to unmask] or 




847-615-7100 ext.2815
-----------------------------------------------------


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 



for additional information, or contact Keach Sasamori at [log in to unmask] or 



847-615-7100 ext.2815
-----------------------------------------------------



PLEASE NOTE: The preceding information may be confidential or
privileged. It only should be used or disseminated for the purpose
of conducting business with Parker. If you are not an intended
recipient, please notify the sender by replying to this message and
then delete the information from your system. Thank you for your
cooperation.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 


for additional information, or contact Keach Sasamori at [log in to unmask] or 


847-615-7100 ext.2815
-----------------------------------------------------


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 

for additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 

for additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815
-----------------------------------------------------


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2