Received: |
by ipc.org (Smail3.1.28.1 #2)
id m0wXSTz-000BjaC; Fri, 30 May 97 09:16 CDT |
Encoding: |
45 Text |
Old-Return-Path: |
|
Date: |
Fri, 30 May 97 05:47:17 cst |
Precedence: |
list |
Resent-From: |
|
Resent-Sender: |
|
X-Status: |
|
Status: |
O |
X-Mailing-List: |
|
>From bergdi Fri May 30 09: |
18:15 1997 |
TO: |
|
Return-Path: |
<TechNet-request> |
Resent-Message-ID: |
<"Gfxhc1.0.K7K.s4kZp"@ipc> |
Subject: |
|
From: |
|
X-Loop: |
|
Cc: |
|
From [log in to unmask] Mon Jun 2 09: |
05:53 1997 |
Message-Id: |
|
Parts/Attachments: |
|
|
Hi TechNet:
Two good sources of information on tin whisker phenomena are: the AMP
web page - there is a good technical article that covers tin whiskers;
And chapter 6.7, page 197 of R.J. Klein Wassink's book "Soldering in
Electronics", ISBN # 0-901150-14-2. Both sources give good, simple
summaries of industry knowledge of tin whiskers. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
______________________________ Reply Separator _________________________________
Subject: Tin Whisker
Author: [log in to unmask] at ccmgw1
Date: 5/28/97 1:08 PM
From: Tuan300859
Currently, I have observed some boards with Tin Whiskers growth. The
whiskers seem to grow from the Tin-lead pads(unusual). The phenomenon is
occurred at only one side of the QFP180 component on the board. Here are my
questions:
1. What is/are the root cause(s) of the Tin Whisker?
2. Are there experiments or tests that had been done?
3. If no to both questions above, Are there any literature that I can read
up to
help determine the root causes of the Whisker?
Thank you in advance
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
|
|
|