TECHNET Archives

January 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Date:
Tue, 29 Jan 2008 14:59:01 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Subject:
From:
"Wenger, George M." <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (108 lines)
It sound like you're assuming that "Champagne voids" ar
Richard,



It sound like you're assuming that "Champagne voids" are "Kirkendahl

voids".  That may be an incorrect assumption.  I've seen "Champagne

voids" in optical micrographs of cross sectioned solder joints but the

only images I seen of "Kirkendahl voids" have been high magnification

SEM images.





Regards, 

George 

George M. Wenger 

Senior Principle FMA / Reliability Engineer 

CommScope / Andrew Wireless Solutions 

40 Technology Drive, Warren, NJ 07059 (908) 546-4531

[log in to unmask] 





-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.

Sent: Tuesday, January 29, 2008 2:31 PM

To: [log in to unmask]

Subject: Re: [TN] Microvoids immersion silver



Werner and Don.

I was always under the impression that Kirkendahl voiding was a result

of the noble metal's (in this case, silver) nucleation through the SJ. I

always thought that this was a time-variable migration. I understand how

all of the process variables described in Werner's  response will affect

or support the eventual void formation, but I would not expect Gaby to

find anything in microsections taken immediately after soldering. Would

it not make more sense to thermally cycle the SJs in order to facilitate

the nucleation prior to microsectioning?



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /*

Sent: Tuesday, January 29, 2008 12:35 PM

To: [log in to unmask]

Subject: Re: [TN] Microvoids immersion silver



Hi Gaby,

I take it what you are seeing are 'champagne voids.'

Voids like these are 'encouraged by rough topography copper, excessive

Ag thickness, some solder paste choices and rapid cool-down after

reflow. But as Donald Cullen says in his comprehensive paper, it

"requires the "Perfect Storm" 

of a rather contrived combination of parameters" to produce planar

micro-voiding.

Well Gaby, now you know it-you are "Perfect." ;-)







Werner







**************

Start the year off right.  Easy ways to stay in shape.

     

http://body.aol.com/fitness/winter-exercise?NCID=aolcmp00300000002489



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To

unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or

(re-start) delivery of Technet send e-mail to [log in to unmask]: SET

Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the

posts: send e-mail to [log in to unmask]: SET Technet Digest Search the

archives of previous posts at: http://listserv.ipc.org/archives Please

visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for

additional information, or contact Keach Sasamori at [log in to unmask] or

847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To

unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or

(re-start) delivery of Technet send e-mail to [log in to unmask]: SET

Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the

posts: send e-mail to [log in to unmask]: SET Technet Digest Search the

archives of previous posts at: http://listserv.ipc.org/archives Please

visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for

additional information, or contact Keach Sasamori at [log in to unmask] or

847-615-7100 ext.2815

-----------------------------------------------------



------------------------------------------------------------------------------------------------

This message is for the designated recipient only and may

contain privileged, proprietary, or otherwise private information.  

If you have received it in error, please notify the sender

immediately and delete the original.  Any unauthorized use of

this email is prohibited.

------------------------------------------------------------------------------------------------

[mf2]



---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2