"BAD idea for just the reasons Paul talks about"

Steve , no need to insult Dough by callin him Paul .

Otherwise, just to make you true ,
Paul talks same as you two,
all sticks (without glue),
check the archives (too),

Not only for the technical reasons ,
on cost side to throw an extra process to equations (cost and complex) just
to "fix"
(sorry Jorge, i know life is not easy, not mothering, ok)
a process is an untidy, laborious, slow, costly, etc. way on DS,
especially considering the dot sizing repeatability difficulties on 603's
(Inge could testify).
To say there is ANY level of assurance of polymer and flux not mixing up on
small items is in practice very ambitious.
Considering, than it is very much understandable sir swami goes to fits upon
seeing the mess underneath ;
the process swami looses 750 cards, acc swami $75OO, and gm swami his cool .
Whole picture entirely unwise , however common .

Only my practiced opinion (don't shoot Jorge)                  paul

PS

Murugan ; for reasons of adhesion (not stoning) on large items (if) ;
this makes perfect sense . Still , research, some heavy packs hold well
upside on steady chain = do you really need it?
Once when mask proved to be too slippery i got under pattern of via holes
(unplated are dearer[better] as secondary drill),
to anchor the adhesive sufficiently for vibro test (finding what holds =
glue[either side] or joint).
Or you can anchor with dispensing paste (less mess than glues)if you have
some brass to tie down .
Really, all 's in application .
Run it without glue ,(if) it falls off , than wonder .
Check yo oven too, may be one of the ersa wonders with chiller on bottom
side in reflow sector ,
than nothing falls off (nothing reflows either if yo chill too high ,
hehehe).
Mind you , we've never had to run the chiller yet (apart from
validations).........


-----Original Message-----
From: Stephen R. Gregory [mailto:[log in to unmask]]
Sent: Wednesday, 16 February 2000 4:15
To: [log in to unmask]
Subject: Re: [TN] Cure and Reflow


In a message dated 02/15/2000 10:29:12 AM Central Standard Time,
[log in to unmask] writes:

<< From my experience with troubleshooting client's processes, it is a very
bad
 idea.  You have too great a chance of mixing curing or outgassing products
 from the adhesive with flux residues from the paste.  The two residues can
 interact with each other to form a detrimental combination.  I published
two
 case studies on a common detrimental effect in my Process Rx column in
 Circuits Assembly magazine - "Microcanyons" and "Become one with the Glue".

 Doug Pauls
 Technical Director, CSL >>

I have to agree with Doug. We had a board at a past employer some years back
which had some problems with the lay-out of components on the
bottomside...the SOT's in particular. We were experiencing a lot of defects
(no solder mostly) on the leads of the SOT's because of the orientation.

Well, it was decided to print solderpaste, dispense glue, place the parts,
and cure and reflow at the same time, with the thought being that we would
make sure that there would be a solder fillet at those troublesome SOT's and
not have to depend on the wave to form them...seemed like a good idea at the
time.

But as we discovered, it was a really BAD idea for just the reasons Paul
talks about. Another thing, which what really caught our customers eye and
got everybody looking at the issue, was that during reflow, during the hot
slump of the paste (and all pastes do hot slump to some degree) the paste
would slump into the epoxy and embed itself into the epoxy...you would
wind-up with all these little solderballs in the epoxy. That was the first
thing that was noticed and started everybody looking at the whole issue.

As a result, the customer rejected all the boards we built doing that,
rework
was out of the question, so we had to eat 750 boards...wasn't too tasty
either.

-Steve Gregory-

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################