Ioan: I have used a solution of sodium rhodizonate. It's made up at 0.2%
BW in a slightly acid(pH 2-3)buffer solution. You can soak the swab in
this and apply to the test sample.
If lead is present it will form a reddish color. This is a qualitative,
not a quantitative test.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
Sent: Wednesday, May 30, 2007 7:07 AM
To: [log in to unmask]
Subject: [TN] Lead test kits
Dear everybody,
I am looking for those handy quick lead testing kits, cotton swab that
turns red or purple if the lead is there. I find a large variety and a
whole lotta suppliers, with prices between 19 and 25$.
I find it very expensive to spend about 20$ for 8 cotton swabs, so maybe
the chemists around here can advise on whether I can do something
in-house, like buying the chemical substance (sodium sulfide?) only.
Thanks,
Ioan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
This message (including any attachments) contains confidential
and/or proprietary information intended only for the addressee.
Any unauthorized disclosure, copying, distribution or reliance on
the contents of this information is strictly prohibited and may
constitute a violation of law. If you are not the intended
recipient, please notify the sender immediately by responding to
this e-mail, and delete the message from your system. If you
have any questions about this e-mail please notify the sender
immediately.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|