TECHNET Archives

1996

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Received:
by ipc.org (Smail3.1.28.1 #2) id m0uMisw-0000EkC; Thu, 23 May 96 17:29 CDT
Old-Return-Path:
Date:
23 May 1996 15:32:27 -0700
Precedence:
list
Resent-From:
Message-ID:
X-Status:
Status:
O
X-Mailing-List:
<[log in to unmask]> archive/latest/4321
From [log in to unmask] Wed Jun 5 11:
18:16 1996
TO:
"IPC Technet" <[log in to unmask]>
Return-Path:
<TechNet-request>
Resent-Message-ID:
<"e-hTZ1.0.lFK.DREfn"@ipc>
Subject:
From:
"Ralph Hersey" <[log in to unmask]>
Resent-Sender:
TechNet-request [log in to unmask]
X-Mailer:
Mail*Link SMTP-QM 3.0.2
X-Loop:
Parts/Attachments:
text/plain (40 lines)
Mail*Link(r) SMTP               FWD>Laminate Voids

<[log in to unmask]> inquired about "laminate voids" with the
following:
 
>We are looking for some help with a processing anomaly which surfaced 
> ~ six months ago. We began to see laminate voids in our epoxy boards. 
>Polyimide does not seem to be affected. We have verified lamination 
>cycles, investigated layer clean, oxide thickness and pre-clean. 
>Solutions seem to remain random. We are running low on ideas. 
     
>Has anyone out there experienced the same problems? Solutions? Riston 
>residues? Conversion coatings?

>From: [log in to unmask]

You probably have volatiles absorbed (moisture or solvent(s)) in the base
(core) material or in the prepreg.

If you have subsurface voids, in your cross sections you should be able to
tell if the voids are in the core or prepreg

If the voids are in the core material, then it is a supplier problem.

If the voids are in the pregreg layers of the printed board then it can be
either a core or prepreg material problem.  In both cases, volatilize-out the
materials prior to lamination using some form of desiccation such as heat
and/or vacuum.  

If the voids are surface and you are foil laminating, you most probably have
volitles in the prepreg and need to desiccate as above.

Ralph Hersey
e-mail:  [log in to unmask]