TECHNET Archives

April 2005

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Guenter Grossmann <[log in to unmask]>
Date:
Fri, 15 Apr 2005 09:38:23 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Vladimir Igoshev <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
Vladimir Igoshev <[log in to unmask]>
Parts/Attachments:
text/plain (82 lines)
Well, it may be not that straight forward calculation. We know that there are 2 of them - Cu6Sn5 (which forms first) and Cu3Sn and each one has its own activation energy.

Regards,

Vladimir

Vladimir Igoshev, Ph. D.
Senior Materials Researcher
Research in Motion
451 Phillip St.
Waterloo, ON, N2L 3X2

Voice: (+1) 519-888-7465, ext. 5283
Fax: (+1) 519-886-0863
E-mail: [log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Guenter Grossmann
Sent: Friday, April 15, 2005 5:34 AM
To: [log in to unmask]
Subject: [TN] Antw: Re: [TN] ENIG - no more problems? / Sn plating


Phil, John

I looked a bit in good ol' Klein Wassink and found his formula for the
growth of intermetallic compounds on Cu surfaces:

d=10^3(exp(-5*10^3/T)t^1/2

d= Thickness of IMC in um
T= Temperature in K
t= time in sec.

The equation can easily be solved for t. Gives a nice Excel spreadsheet
where the time for a given temperature can be estimated a layer of Sn of
a certain thickness needs to be transformed to IMC and will thus make
problems  in soldering. Gives interesting results when Sn 0.8um is
compared with 1.2um thickness.

Guenter



EMPA
Swiss Federal Laboratories  for Materials Testing and Research
Centre for Reliability
Guenter Grossmann,  Senior Engineer

8600 Duebendorf
Switzerland

Phone: xx41 1 823 4279
Fax :     xx41 1 823 4054
mail:     [log in to unmask]

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------



---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2