Hi All,
Mike Weekes thread kinda' ties into my thread last week about dewetting cap
acitors...
I got my corrective action report from the manufacturer, and they acknowleged
that there was insufficient nickel barrier plating. Their minimum nickel
thickness is called out to be a minimum of 50-micro-inches, some of the caps that
I sent them from the reel, measured down around 6-micro-inches. They have an
explanation of how this could have happened, and what they have done to prevent
this from occuring in the future, but I'm still wondering about reliabilty...
I was told over the phone that if they wet with solder, they would be
fine...but I don't have anything documented from them that states that...
How important is the barrier plating on capacitor terminations to reliabilty?
Should I ask them to document that there will be no reliabilty concerns with
the capacitors that came from this lot that have shown visually good solder
wetting?
Still don't have a "warm and fuzzy" about all this...
-Steve Gregory-
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|