TECHNET Archives

August 2013

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Joyce Koo <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Joyce Koo <[log in to unmask]>
Date:
Thu, 8 Aug 2013 12:55:51 +0000
Content-Type:
text/plain
Parts/Attachments:
text/plain (162 lines)
"I haven't seen any published data on that aspect of QFNs so it may not be a significant issue." - hmmm, not sure if it is valid assumption.  Not when you have lawyers and legal department review your paper.  How long you have to wait for the corona arcing to be published?  Tin/zinc Whiskers on electronics? 10 to 20 years? Dave, you are very courageous. (even without lawyers, did you see start up publish defect tracking data? Even less than the lawyer reviewed one).  

Joyce Koo
Researcher
Materials Interconnect Lab
Office: (519) 888-7465 79945
BlackBerry: (226) 220-4760

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Thursday, August 08, 2013 8:40 AM
To: [log in to unmask]
Subject: Re: [TN] QFN solder voiding

Hi Bryan - concerning the voiding of the center pad, I'll have to steal 
Doug's answer of "it depends". We use a requirement of 50% maximum void 
unless there is a functional circuit requirement  such as grounding or 
thermal. As a number of TechNet folks have detailed, there are various 
ways to easily achieve that 50% maximum void. There are always going to be 
some voiding but we routinely keep the voiding under 25% of the center pad 
area. Out of the couple 100 QFN packages we deal with, there has only been 
two cases where the 50% maximum requirement wasn't sufficient. We made 
stencil adjustments to insure we hit a 20% maximum value and the QFN 
packages were suddenly very happy (both cases involved signal grounding). 
As you mentioned, the peripheral pads are a whole other story and I 
suspect voids have a bigger impact there - I haven't seen any published 
data on that aspect of QFNs so it may not be a significant issue. There 
were some very good papers at the 2012 SMTAI conference on QFNS which 
would be useful too. Good luck with  your process development.

Dave



From:   "Kerr, Bryan (UK)" <[log in to unmask]>
To:     <[log in to unmask]>
Date:   08/08/2013 02:55 AM
Subject:        Re: [TN] QFN solder voiding
Sent by:        TechNet <[log in to unmask]>



Hi All

Thanks for all the responses. I'm sure that in most cases we have little 
choice but to develop our processes to suit these problematic component 
styles however I think the aspirations of the expected soldering standards 
vary considerably. I think there is a general acceptance that 50% coverage 
of the base is enough although some people, customers and component 
suppliers, are beginning to demand more. Peripheral pads are not specified 
within any standard I know of and these can show a level of voiding too so 
this still needs to be developed.

Bryan

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: 08 August 2013 01:12
To: [log in to unmask]
Subject: Re: [TN] QFN solder voiding

----------------------! WARNING ! ---------------------- This message 
originates from outside our organisation, either from an external partner 
or from the internet.
Keep this in mind if you answer this message.
Follow the 'Report Suspicious Emails' link on IT matters for instructions 
on reporting suspicious email messages.
--------------------------------------------------------

Preform.

From: [log in to unmask]
Sent: Wednesday, August 7, 2013 7:47 PM
To: [log in to unmask]
Reply To: TechNet E-Mail Forum
Subject: Re: [TN] QFN solder voiding


Steve and all others.
 Void free center pads are achievable but you have to really think out of 
the box to arrive at a solution. I have worked with parts 1.6mm square to 
parts as large as a postage stamp and the same basic techniques work.

Helpful hints;
Solder mask is your enemy and the proper aperture will look very different 
than what you usually see.
 Little blocks of solder paste will only result in voids.
Think out of the box.

Due to my work I really cannot reveal the secrets but the results can be 
achieve.

John

 On Wed, 7 Aug 2013 14:12:02 -0600, Steve Gregory <[log in to unmask]>
wrote:
> (background chorus) I want my...I want my...parts void free!
>
> Steve
>
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Whittaker, Dewey
> (EHCOE)
> Sent: Wednesday, August 7, 2013 1:47 PM
> To: [log in to unmask]
> Subject: Re: [TN] QFN solder voiding
>
> Striking a familiar chord; Excellent!
> Dewey
________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential 
information, privileged material (including material protected by the 
solicitor-client or other applicable privileges), or constitute non-public 
information. Any use of this information by anyone other than the intended 
recipient is prohibited. If you have received this transmission in error, 
please immediately reply to the sender and delete this information from 
your system. Use, dissemination, distribution, or reproduction of this 
transmission by unintended recipients is not authorized and may be 
unlawful.

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

********************************************************************
This email and any attachments are confidential to the intended
recipient and may also be privileged. If you are not the intended
recipient please delete it from your system and notify the sender.
You should not copy it or use it for any purpose nor disclose or
distribute its contents to any other person.
********************************************************************

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________




______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2