TECHNET Archives

August 2009

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Inge <[log in to unmask]>
Date:
Mon, 24 Aug 2009 23:38:49 +0200
Content-Type:
text/plain
Parts/Attachments:
text/plain (69 lines)
Thanks Ken,
are there any stds that demand a perfect surface, e.g. any IPC standards. 
And what use to cause outgassing issues? I have several PWB courses behind, 
but many, many years ago. Can dig in my piles, but a faster answer from TN 
seems a bit more comfortable.
/Inge


----- Original Message ----- 
From: "Ken Bloomquist" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Monday, August 24, 2009 11:20 PM
Subject: Re: [TN] Manual spraying, further qs


> The bad board had beans for lunch, "bad out gassing problem"! :-)
>
> KennyB
>
> -----Original Message-----
> From: Inge [mailto:[log in to unmask]]
> Sent: Monday, August 24, 2009 1:50 PM
> To: [log in to unmask]
> Subject: Re: [TN] Manual spraying, further qs
>
> This very day, I couldn't stay aside but had to do something to help the
> production guys. So, I took a fresh, naked and qualified board from 
> another
> source and did this:
> Put one of our problem boards beside the reference board, both on bottom 
> of
> a larg well box, i.e. no fans blowing, nor any evacuation. Sprayed both
> simultaneosly. Inspected them after one hour at room  temp. The reference
> board was absolutely perfect, while the other was matte! Had a look in a
> microscope. The bad guy had thousands of microscopic inclusions and even
> superficial voids, the reference was perfect. Noticed that the bad boards
> have a much coarser (looks like the net pattern after screen 
> printing)green
> sheet (solder mask) and numerous voids already before spraying. What is 
> your
>
> opinion?
> /Inge
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
> for additional information, or contact Keach Sasamori at [log in to unmask] or 
> 847-615-7100 ext.2815
> ----------------------------------------------------- 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2