TECHNET Archives

October 2010

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Steve Gregory <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Date:
Wed, 27 Oct 2010 09:35:17 -0400
Content-Type:
text/plain
Parts/Attachments:
text/plain (102 lines)
Hi Guenter,

Your pictures are now up:

http://stevezeva.homestead.com/P_2a.jpg

http://stevezeva.homestead.com/P_2b.jpg

http://stevezeva.homestead.com/SaiaNr2_CS6_End_of_crack.jpg

http://stevezeva.homestead.com/SaiaNr2_7_short_failure.jpg

Steve

-----Original Message-----
From: Grossmann, Guenter [mailto:[log in to unmask]] 
Sent: Wednesday, October 27, 2010 8:14 AM
To: Steve Gregory
Subject: AW: [TN] Cracks in BGA solderjoints

Hi Steve

Thanks for your help

Günter 


>-----Ursprüngliche Nachricht-----
>Von: Steve Gregory [mailto:[log in to unmask]]
>Gesendet: Mittwoch, 27. Oktober 2010 13:08
>An: 'TechNet E-Mail Forum'; Grossmann, Guenter
>Betreff: RE: [TN] Cracks in BGA solderjoints
>
>Hi Guenter,
>
>If you send the pictures to me I'll put them up on my web page then 
>post the link so everyone can see them.
>
>Steve Gregory
>
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]] On Behalf Of Grossmann, Guenter
>Sent: Wednesday, October 27, 2010 3:37 AM
>To: [log in to unmask]
>Subject: [TN] Cracks in BGA solderjoints
>
>Hi Technetters
>
>I have an effect in BGA solder joints that I have never seen before.
>In microsections and in FIB preparations I see cracks between the IMC 
>and a slightly darker region towards the Ni which I assume to be a P 
>enriched zone of the Ni. However, the cracks are somewhere in the width 
>of the solder joint and they are quite short running out to a row of 
>pores that look somehow like Kirkendall voids.
>Is there still a possibility to place one or two pictures? Kim's IPC 
>site doesn't work.
>
>Best regards
>
>Günter
>
>
>
>______________________________________________________________________
>This email has been scanned by the MessageLabs Email Security System.
>For more information please contact helpdesk at x2960 or 
>[log in to unmask] 
>______________________________________________________________________
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0 To 
>unsubscribe, send a message to [log in to unmask] with following text in 
>the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt 
>or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing 
>per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
>http://listserv.ipc.org/archives
>Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] 
>or 847-615-7100 ext.2815
>-----------------------------------------------------



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2