TECHNET Archives

December 2013

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
"Wenger, George M. [Contractor]" <[log in to unmask]>
Date:
Tue, 24 Dec 2013 10:59:23 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Message-ID:
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
TechNet E-Mail Forum <[log in to unmask]>
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (394 lines)
Hi George - so you are advocating "QFN insanity in small doses?"?

Dave



From:   "Wenger, George M. [Contractor]" <[log in to unmask]>
To:     TechNet E-Mail Forum <[log in to unmask]>, 
"[log in to unmask]" <[log in to unmask]>
Date:   12/24/2013 10:41 AM
Subject:        RE: [TN] IPC-A-610E, Voids in Thermal exposed pad of QFNs



It looks like I'm in the middle between Dave and Richard.  I agree with 
Richard's statement if you put a qualifier at the end of the statement 
(i.e., "QFNs should not be used in hi-reliability devices" if you have an 
alternative).  And I agree with Dave that QFNs are very reliable 
components when you add several qualifiers at the end of his statement as 
he indicates (i.e., you need to understand the component technology, 
qualify and monitor your assembly process).

If I were a component vendor I'd like everyone to use QFNs because it 
gives me advantages.  If I were solder process assembly engineer I'd 
rather have a component package that didn't require as much of my time as 
QFNs do.  However, we need to be pragmatic and realize that QFNs are here 
and aren't going away and their use is increasing and we need live with 
them.

Regards,
George
George M. Wenger
Failure Signature & Characterization Lab LLC
609 Cokesbury Road, High Bridge, NJ 08829
(908) 638-8771 Home (732) 309-8964 Mobile
E-mail: [log in to unmask]
[log in to unmask]

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Tuesday, December 24, 2013 11:06 AM
To: [log in to unmask]
Subject: Re: [TN] IPC-A-610E, Voids in Thermal exposed pad of QFNs

Hi Richard - you and I are on the same page except for the "QFNs should 
not be used in hi-reliability devices". Are QFNs a complex technology to 
understand? Absolutely, but if you do your homework and put into place the 
correct process controls, QFNs are very reliable components (the IPC-7093 
standard is a good starting point). The NASA DoD consortia study 
demonstrated that QFNs were a very reliable component technology under 
high performance equipment test conditions. The voiding associated with 
QFNs should be handled no differently than the voiding associated with 
BGAs -  we need to understand why the voids are present, what possible 
impact the voids could have on the QFN component, and what steps need to 
be taken to have a process that produces an acceptable level of voiding 
(which can be wide range of acceptability). I think the point of the 
entire QFN/void thread has been that QFNs need to be understood as a 
component technology or just don't put them on your assembly.

Happy Holidays!

Dave



From:   "Stadem, Richard D." <[log in to unmask]>
To:     <[log in to unmask]>
Date:   12/23/2013 04:48 PM
Subject:        Re: [TN] IPC-A-610E, Voids in Thermal exposed pad of QFNs
Sent by:        TechNet <[log in to unmask]>



Nobody has responded to the fact that you cannot validate you actually 
have surface-to-surface wetting in the non-voided areas of QFNs and other 
SMT components with belly pads. The point I am trying to make is that QFNs 
really should not be used in hi-reliability devices. I know they are, but 
they present so many issues, and chief amongst them is cases like 
Reuven's, where a total amount of voiding of 25% maximum is required by 
his customer.

There is no way to validate compliance to that requirement.

The entire surface of the board pad could be covered with solder with no 
voiding visible in the X-ray, but none of the solder may actually be 
wetted to the bottom of the part. I have seen this happen many times; I 
was called in to determine what the reliability issue was with some QFNs 
overheating, and others not, and the client was puzzled because the ones 
that failed did not show any evidence of voids, they were completely 
opaque. They did not show any evidence of voiding because there was little 
or no wetting to the bottom of the QFN, only to the board pad, therefore 
no heat-sinking whatsoever.

Voids only appear on belly pad solder joint X-rays if at least some of the 
solder is wetted to both the bottom of the part and to the pad on the PWB.
From this experience, if I see a QFN belly pad solder joint without any 
voids at all, I immediately suspect there is no solder contact whatsoever, 
not the opposite. To me, voiding manifest in the X-rays of QFN solder 
joints is a good thing, as it indicates solder wetting took place on both 
surfaces.

Now, if components fail because the amount of voiding is greater than 25% 
and you cannot guarantee your process will always provide less than 25% 
voiding, that is a design issue, not a process capability issue. Design 
engineers should take note of that.

I would bill extra for the rework that is going to happen to meet that 
particular requirement.

From: Reuven Rokah [mailto:[log in to unmask]]
Sent: Monday, December 23, 2013 10:04 AM
To: Stadem, Richard D.
Cc: TechNet E-Mail Forum
Subject: Re: [TN] IPC-A-610E, Voids in Thermal exposed pad of QFNs

Hi Richard,
If you design the thermal pad by dividing its area to small thermal pads 
you will improve the air escape possibility during the soldering process, 
reduce the voids creation and increase wetting.
Same you have to design the stencil and its thickness accordingly.
Still I am recommending to add requirements for the Power QFN voids.

On Mon, Dec 23, 2013 at 5:30 PM, Stadem, Richard D.
<[log in to unmask]<mailto:[log in to unmask]>> wrote:
The amount of voiding in this type of part has to be directed as a 
percentage of the possible overall wetting.
Some EMS assemblers purposely reduce the amount of solder volume to ensure 
the periphery leads fully wet (no pendulum effect) and to avoid solder 
balls under the part, which is a common problem with QFNs. So, if you only 
have wetting over 50% of the belly pad, you may need to have a reduced 
amount of voiding to correspond to protect the reliability of the solder 
connection and the thermal transfer or current carrying capacity.
Instead of looking at the amount of voiding, it may be better to have a 
general requirement for the minimum amount of wetting. Now, having said 
that, how do you propose to ensure that the minimum amount of wetting is 
actually accomplished?
Are the non-voided areas you see in the X-ray really wetted both to the 
bottom of the component and the top of the board pad? You cannot assume 
that. How do you know? Not even laminar X-ray (5DX or similar) can prove 
full surface-to-surface wetting beyond the "shadow of a doubt". All you 
see are shadows.

Check this out:  http://www.youtube.com/watch?v=owbgPVOQlbY


-----Original Message-----
From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf 
Of Reuven Rokah
Sent: Friday, December 20, 2013 10:18 AM
To: [log in to unmask]<mailto:[log in to unmask]>
Subject: Re: [TN] IPC-A-610E, Voids in Thermal exposed pad of QFNs

Hi All,
I started with this issue because of my customer needs (max 25% voids) and 
argue with the EMS (one one the biggest) that its guide lines require 40% 
maximum of voids.
In my opinion it should be included in the IPC-A-610 such as class 1, 2, 3 
and above class 3 such as 10% voids (using vapor phase), should be agreed 
between the two sides.


On Fri, Dec 20, 2013 at 3:04 PM, David D. Hillman < 
[log in to unmask]<mailto:[log in to unmask]>> wrote:

> Hi Joyce - sometimes we can get too technical and over think a
component.
> As you detailed, there can be a number of inputs to the equation but
> not necessarily. We have been using the 50% maximum void rule for 5
> years on QFNs  and I have only 2 cases where we had either a thermal
> or grounding issue that required us to maintain a smaller voiding
> percentage of the thermal pad.
>
> Dave
>
>
>
> From:   Joyce Koo <[log in to unmask]<mailto:[log in to unmask]>>
> To:     'TechNet E-Mail Forum' <[log in to unmask]<mailto:[log in to unmask]
>>,
> "[log in to unmask]<mailto:[log in to unmask]>'"
<[log in to unmask]<mailto:[log in to unmask]>>
> Date:   12/20/2013 06:45 AM
> Subject:        RE: [TN] IPC-A-610E, Voids in Thermal exposed pad of
QFNs
>
>
>
> Correct me if I am wrong, as for the thermal goes, there are many
> factors just the voiding.  For example, the requirements of heat
> transfer path - vertical vs side, MCM possibly will have multiple
> grounds that may required isolation of heat path.  If you allow 50%
> voids, depend upon the thermal via path, you might missing one sector
> of the MCM heat conduction path all together (if it is vertically
> channeled).  It is not as easy as a single number.  It is a bit of
> scary when the design is so far above the supply chain.
>
> Joyce Koo
> Researcher
> Materials Interconnect Lab
> Office: (519) 888-7465 79945
> BlackBerry: (226) 220-4760
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On
> Behalf
Of David D. Hillman
> Sent: Friday, December 20, 2013 7:36 AM
> To: [log in to unmask]<mailto:[log in to unmask]>
> Subject: Re: [TN] IPC-A-610E, Voids in Thermal exposed pad of QFNs
>
> Hi Reuven - I think that is a possible idea, however, what void
> percentage
>
> do you suggest and what technical data/investigative studies do you
> have to support the recommended void percentage? One thing to consider
> is that if a workmanship topic is missing from the JSTD-001/IPC-610
> documents, it doesn't mean that the topic hasn't been reviewed.  The
> IPC committees work
>
>  hard to only put workmanship criteria in the specifications that is
> necessary and is supported by data. An example - the IPC-7093 BTC
> committee completed extensive efforts looking at the voiding of QFN
> thermal pads and found no industry consensus on a void percentage
> requirement. The JSTD-001 committee therefore has not included a
> maximum void percentage requirement in the 001 specification and the
> IPC-610 specification shows no examples of voiding requirements of QFN
> thermal pads. The workmanship criteria show in the JSTD-001/IPC-610
> specifications
>
> results in added costs to products and processes so the committees are
> very careful to not add requirements unless there is technical
> data/justification. I know a number of OEMs/CEMS who have a 50%
> maximum void requirement on the QFN thermal pad unless the component
> has specific thermal or electrical functional requirements. The
> IPC-7093 specification has some good information on the topic of BTC
> thermal pads and voids. The committees would welcome any investigative
> data on the topic too.  Happy Holidays!
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]<mailto:[log in to unmask]>
>
>
>
> From:   Reuven Rokah <[log in to unmask]<
mailto:[log in to unmask]>>
> To:     <[log in to unmask]<mailto:[log in to unmask]>>
> Date:   12/20/2013 12:48 AM
> Subject:        [TN] IPC-A-610E, Voids in Thermal exposed pad of QFNs
> Sent by:        TechNet <[log in to unmask]<mailto:[log in to unmask]>>
>
>
>
> Hi TechNets,
>
> I didn't see in the IPC-A-610E any acceptability reference in regards
> with the percentage of voids in solder joints of exposed thermal pads
> of QFNs or other components with exposed thermal pads.
>
> I recommend to add it in the next revision.
>
>
> --
>
> Best Regards,
>
> *Reuven Rokah*
>
> Mobile: 972-52-6012018
> Tel:        972-3-9360688
> Fax:          076-5100674
>  <http://www.rokah-technologies.com/>[log in to unmask]<
mailto:[log in to unmask]>
> [log in to unmask]<mailto:[log in to unmask]>
> www.rokah-technologies.com<http://www.rokah-technologies.com>
>
>
> This e-mail message is intended for the recipient only and contains
> information which is CONFIDENTIAL and which may be proprietary of
> RokahTechnologies. If you have received this transmission in error,
> please inform me by e-mail, phone or fax, and then please delete all
> of the original files and all other copies exist.
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud
service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]<mailto:[log in to unmask]>
> ______________________________________________________________________
>
>
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud
service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]<mailto:[log in to unmask]>
> ______________________________________________________________________
> ---------------------------------------------------------------------
> This transmission (including any attachments) may contain confidential
> information, privileged material (including material protected by the
> solicitor-client or other applicable privileges), or constitute
> non-public information. Any use of this information by anyone other
> than the intended recipient is prohibited. If you have received this
> transmission in error, please immediately reply to the sender and
> delete this information from your system. Use, dissemination,
> distribution, or reproduction of this transmission by unintended
> recipients is not authorized and may be unlawful.
>
>
>
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud
service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]<mailto:[log in to unmask]>
> ______________________________________________________________________
>



--

Best Regards,

*Reuven Rokah*

Mobile: 972-52-6012018
Tel:        972-3-9360688
Fax:          076-5100674
 <http://www.rokah-technologies.com/>[log in to unmask]<
mailto:[log in to unmask]>
[log in to unmask]<mailto:[log in to unmask]>
www.rokah-technologies.com<http://www.rokah-technologies.com>

This e-mail message is intended for the recipient only and contains 
information which is CONFIDENTIAL and which may be proprietary of Rokah 
Technologies. If you have received this transmission in error, please 
inform me by e-mail, phone or fax, and then please delete all of the 
original files and all other copies exist.

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]< 
mailto:[log in to unmask]> 
______________________________________________________________________



--
Best Regards,

Reuven Rokah

Mobile: 972-52-6012018
Tel:        972-3-9360688
Fax:          076-5100674
<http://www.rokah-technologies.com/>[log in to unmask]
<mailto:[log in to unmask]>[log in to unmask]<
mailto:[log in to unmask]>
www.rokah-technologies.com<http://www.rokah-technologies.com/>

[http://royiro.weebly.com/uploads/6/3/6/9/6369812/4511319.jpg?303]
This e-mail message is intended for the recipient only and contains
information which is CONFIDENTIAL and which may be proprietary of Rokah
Technologies. If you have received this transmission in error, please
inform me by e-mail, phone or fax, and then please delete all of the
original files and all other copies exist.

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________




______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________




______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2