I would heed the gold embrittlement caution. You can have good
solderability but that does not mean the solder joint will be reliable. I
have witnessed boards that appear to have good solderability (maybe a
little grainy) but if you flex or twisted the board you would hear
cracking and some of the parts would actually fall off.
Joel Alexander
Quality Assurance Manager
TT APSCO, INC.
[log in to unmask]
Sent by: TechNet <[log in to unmask]>
03/15/2007 07:32 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]
To
[log in to unmask]
cc
Subject
Re: [TN] IPC ENIG SPECIFICATION
Thanks for the prompt reply. I can do the gold calculations - lots of
stuff on the tech-net telling me how to do that. We have not seen any
solderability issues. I would still like an explanation of the reasoning
behind the minimum nickel thickness( besides a keypad type application).
Regards Steve Kelly>
Steve,
>
> I will likely solder quite well, but the gold is quite thick for
> soldering to without incurring the wrath of gold embrittlement. I would
> not be so concerned about the thin nickel as the overabundance of gold.
>
> If the gold were nice and soft, it would be nice for gold ball bonding!
> But, the nickel is quite thin.
>
> If the numbers are correct, you did not receive ENIG - have them sent
> back
>
> Steve C
>
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|