TECHNET Archives

June 2011

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Steve Gregory <[log in to unmask]>
Date:
Thu, 9 Jun 2011 11:19:50 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Gary Robinson <[log in to unmask]>
Message-ID:
Subject:
From:
Gary Robinson <[log in to unmask]>
X-cc:
TechNet E-Mail Forum <[log in to unmask]>
In-Reply-To:
<004a01cc26bf$e815bed0$b8413c70$@com>
Content-Type:
text/plain; charset="ISO-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (250 lines)
Too all - thanks for the input - there is very good dialog that will help us
understand what is going on here and I appreciate everyones comments.

On Thu, Jun 9, 2011 at 11:11 AM, Steve Gregory <[log in to unmask]>wrote:

> Hi again Gary,
>
> Here's the additional photos that you sent me:
>
> http://stevezeva.homestead.com/good_joint.jpg
>
> http://stevezeva.homestead.com/Good_Joint_next_to_bad.jpg
>
> http://stevezeva.homestead.com/Via_and_Black_PTH_1.jpg
>
> http://stevezeva.homestead.com/Black_PTH_2.jpg
>
> http://stevezeva.homestead.com/Black_Unwetted_PTH__Post_Wave.jpg
>
> Steve
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Gary Robinson
>  Sent: Thursday, June 09, 2011 11:19 AM
> To: [log in to unmask]
> Subject: Re: [TN] Black Pad?
>
> We run a blank board but it is from a different Lot code and appears to
> solder fine.
> Maybe we try an run one through reflow oven then wave?
>
> To answer some of the other questions -
> Both profiles are in spec
> Reflow Peak at 244 - TAL - 88sec
> overall time is 5 min ramp to peak
>
> Wave -
> Ramp to 140 and soak with  .5 Deg/sec increase to 163 for 1.3 min.
> Delta is 10 deg C (big Xfrmr)
> Contact Time - 2.4 Sec
>
>
> On Thu, Jun 9, 2011 at 9:58 AM, Tontis, Theodore <
> [log in to unmask]> wrote:
>
> > Would it be possible to run a bare board through the wave that hasn't
> > been through the reflow process?
> >
> > Ted T.
> >
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
> > Sent: Thursday, June 09, 2011 9:38 AM
> > To: [log in to unmask]
> > Subject: Re: [TN] Black Pad?
> >
> > Steve,
> >
> > I agree with your assessment about possible oxidation of Ni 1st pass and
> > dewetting during wave soldering.
> >
> > Regards,
> > George
> > George M. Wenger
> > Senior Principal Reliability / FMA Engineer
> > Andrew Corporation - Wireless Network Solutions
> > 40 Technology Drive, Warren, NJ 07059
> > (908) 546-4531 Office (732) 309-8964 Mobile
> > E-mail: [log in to unmask]
> >
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
> > Sent: Thursday, June 09, 2011 9:59 AM
> > To: [log in to unmask]
> > Subject: Re: [TN] Black Pad?
> >
> > Hi Gary,
> >
> > I got your pictures this morning, and have them posted now:
> >
> > http://stevezeva.homestead.com/Joint_1.JPG
> >
> > http://stevezeva.homestead.com/Joint_2.JPG
> >
> > http://stevezeva.homestead.com/via.JPG
> >
> > Although the pictures show some non-wetting happening, it's difficult to
> > see
> > what exactly is going on.
> >
> > You say that the component side seems fine, it's just when you're trying
> > to
> > wave solder is when you see the problem. Maybe you have thin gold, and
> > when
> > the boards were fresh, the SMT was able to solder fine. But then after
> > the
> > boards went through reflow, the underlying nickel oxidized so badly that
> > solder wasn't able to wet?
> >
> > Steve
> >
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]] On Behalf Of Gary Robinson
> > Sent: Wednesday, June 08, 2011 4:46 PM
> > To: [log in to unmask]
> > Subject: [TN] Black Pad?
> >
> > We have noticed a problem only on ENIG boards in our WAVE process that
> > looks
> > similar to Black Pad but do not know how to identify or where to begin
> > to
> > find a resolution to the problem.  We were hoping an expert may have
> > experience in seeing this problem.  Here are some facts -
> > 1.  Black residue is on the vias and thts on the solder side. Please see
> > the
> > attached images.
> > 2.  Component Side SMT Parts do not exhibit the same problems.
> > 3.  Boards are processed PbFree - SAC305, Pacific 2009m No Clean Water
> > Based
> > flux
> > 4.  THTs will not wet after residues appear (for touch up process)
> > 5.  Blowholes appear to accompany the defect but are not always present.
> >
> > Thanks for your help in advance.
> >
> >
> > ______________________________________________________________________
> > This email has been scanned by the MessageLabs Email Security System.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 16.0
> > To unsubscribe, send a message to [log in to unmask] with following text
> > in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to
> > [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to
> > [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at:
> > http://listserv.ipc.org/archives
> > For additional information, or contact Keach Sasamori at [log in to unmask]
> > or
> > 847-615-7100 ext.2815
> > -----------------------------------------------------
> >
> >
> > ______________________________________________________________________
> > This email has been scanned by the MessageLabs Email Security System.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 16.0
> > To unsubscribe, send a message to [log in to unmask] with following text
> > in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to
> > [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to
> > [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at:
> > http://listserv.ipc.org/archives
> > For additional information, or contact Keach Sasamori at [log in to unmask]
> > or 847-615-7100 ext.2815
> > -----------------------------------------------------
> >
> > ______________________________________________________________________
> > This email has been scanned by the MessageLabs Email Security System.
> > For more information please contact helpdesk at x2960 or
> > [log in to unmask]
> > ______________________________________________________________________
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 16.0
> > To unsubscribe, send a message to [log in to unmask] with following text
> > in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to
> > [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to
> > [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at:
> > http://listserv.ipc.org/archives
> > For additional information, or contact Keach Sasamori at [log in to unmask]
> > or 847-615-7100 ext.2815
> > -----------------------------------------------------
> >
> > ______________________________________________________________________
> > This email has been scanned by the MessageLabs Email Security System.
> > For more information please contact helpdesk at x2960 or
> [log in to unmask]
> > ______________________________________________________________________
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 16.0
> > To unsubscribe, send a message to [log in to unmask] with following text
> in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to
> > [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to
> > [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at:
> http://listserv.ipc.org/archives
> > For additional information, or contact Keach Sasamori at [log in to unmask]
> > 847-615-7100 ext.2815
> > -----------------------------------------------------
> >
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 16.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> For additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
>


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2