Were the issues with silver plated component issues back i
Dave,
Were the issues with silver plated component issues back in the SMART
conference era diagnosed as solder joint embrittlement by silver because
of too thick a plating or were they termination failures on the silver
plated components. In the RF world silver plating is liked by the
design community because of its electrical properties. However, solder
assembly engineers always have difficulty trying to make reliable solder
joints to components that have upwards of 15 to 20 microns of silver
plating. When you look at the dissolution rate of silver into solder
you realize very quickly that when you try to solder to silver plating
this thick you wind up making a solder joint to the plating and not to
the base metal. So the question really is that when a solder joint made
to thick silver fails why did it fail? Was it due to silver
embrittlement or was it because you made a solder joint to silver rather
than a base metal. If all of the silver isn't dissolved then if you
evaluate the silver content across the termination interface you see
that the silver content in the solder may be a couple of percent but
when you reach the silver plating side of the termination the silver
content is at 100%. One needs to make sure that an analysis of the
failure mode is done in order to classify solder joint failures. I for
one do not believe that silver embrittlement is worst than gold
embrittlement. Certainly I've seen many more solder interconnection
failures on joints made to thick silver plating than I have to ENIG or
even thick 1 micron of gold plating but I've never seen any data
anywhere that shows solder joints made to silver those thickness is 0.05
to 1 micron is any more brittle that solder joints made to 0.05 to 1
micron of gold.
Regards,
George
George M. Wenger
Andrew Corporation Wireless Network Solutions
Senior Principal FMA / Reliability Engineer
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 [Office] (732) 309-8964 [Cell]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Friday, May 25, 2007 12:51 PM
To: [log in to unmask]
Subject: Re: [TN] Silver Embrittlement?
Hi folks! Just a comment. Some of Werner's comments of Ag embrittlement
are based on some ceramic components with silver plated finishes which
resulted in severe solder joint issues on a series of investigations
back
in the SMART conference era. The IPC-4553 Immersion Ag finish group is
in
the final stages of finishing up an investigation where Immersion Ag
surface finish was applied to test vehicles in both 1X and 3X
thicknesses
plus combine with SnPb and Pbfree soldering processes. The goal of the
testing is to characterizes and determine if silver embrittlement of
solder joint can be created under practical applications. The thermal
cycle testing is complete and 100+ cross sections are undergoing SEM
elemental mapping analysis. The report will be completed this year -
keep
an eye on the IPC-4553 group activities.
Dave Hillman
Rockwell Collins
[log in to unmask]
Werner Engelmaier <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
05/25/2007 08:12 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]
To
[log in to unmask]
cc
Subject
Re: [TN] Silver Embrittlement?
Hi Lee,
Au- and Ag-embrittlements are certainly documented?the combined effect
is
simply my extension of the phenomena.
Werner
**************************************
See what's free at http://www.aol.com.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
------------------------------------------------------------------------------------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original. Any unauthorized use of
this email is prohibited.
------------------------------------------------------------------------------------------------
[mf2]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|