Hi Steve! How thick is the pwb? Was the profile right? We typically see the
solder flow stop short of covering the pwb pad when using immersion silver
but not to the extent that your pictures showed. Did you get enough flux
applied to the pwb? The 2331 flux is pretty active and I would have thought
it would move out any oxidation that would be present from the two reflow
passes.
Dave
Stephen Gregory
<Stephen.Gregory@
LABARGE.COM> To
Sent by: TechNet [log in to unmask]
<[log in to unmask]> cc
Subject
03/02/2006 04:15 [TN] As long as we're talking about
PM silver...
Please respond to
TechNet E-Mail
Forum
<[log in to unmask]>
; Please respond
to
Stephen Gregory
<Stephen.Gregory@
LABARGE.COM>
Hi All!
I figured as long as we're talking about silver, you might take a look
at some PTH solder joints on some boards we just built with an immersion
silver finish. I'm posting these pictures because this is the first
production board we've built here that has an ImAg finish, and I would
like to know if this appearance is pretty typical. Go check out:
http://stevezeva.homestead.com/files/Immersion_Silver_PTH.jpg
http://stevezeva.homestead.com/files/Immersion_Silver_PTH_2.jpg
This particular board went through double-sided reflow, and then the PTH
was soldered using a selective wave solder pallet while being fluxed
with an ultrasonic spray fluxer using Kester 2331ZX OA flux.
You can see that the solder didn't flow out to the edges of the pads on
the primary side of the board, the secondary side of the board looks
wonderful. I know this is not a defect according to the -610...but is
this typical? Especially since it went through two reflow cycles?
Thanks in advance!
-Steve Gregory-
_______________________________________________________
This message may contain information that is privileged and confidential to
LaBarge, Inc. It is for use only by the individual or entity named above.
If you are not the intended recipient, you may not copy, use or deliver
this message to anyone. In such event, you should destroy the message and
kindly notify the sender by reply e-mail.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|