text/plain (135 lines)
hi again,

there are no ipc documents, that showed up with my search, regarding plasma etching of kapton (or polyimide).

google was much more rewarding. here is one vendor that is very specific about plasma etching kapton board material.

phil

http://www.plasmaetch.com/innovat.html

-----Original Message-----
From: Dhawan, Ashok [mailto:[log in to unmask]]
Sent: Friday, May 14, 2004 9:32 AM
To: [log in to unmask]
Subject: Re: [TN] Flex Circuit


Phil

The flex circuit has SM Parts besides THT parts. The urethane coating is
required on all of the flex circuit surface except hardware and mounting
areas.

We intend to plasma etch or scrubb ( mech abrade) the PCb prior to assembly.
However, we need to define it and specify it with reference of an industrial
standard such as IPC, J-STD, Mil STd or any other standard.

Do you know any such standard ? Any Aerospace or Mil Standard users
specifying this process for their flex ckts ?

I will appreciate inputs on this .

Regards


Ashok

-----Original Message-----
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Friday, May 14, 2004 11:12 AM
To: [log in to unmask]; [log in to unmask]
Subject: RE: [TN] Flex Circuit


hi,

why would you want to conformal coat the polyimide film on a flex circuit?
basically, it is a conformal coating (only better) if you know what i mean.
would you conformal coat polyimide jacketed wire...probably not. conformal
coating the terminations would make some sense.

as you found out, to get the coating to adhere, requires some mechanical
scrubbing on the polyimide to increase its surface energy as brian of
corsica might say.  if you insist on coating this stuff, you might want to
abrade it before you assemble anything to it.

it's friday, and i'm having fun.

phil

-----Original Message-----
From: Ashok Dhawan [mailto:[log in to unmask]]
Sent: Friday, May 14, 2004 7:39 AM
To: [log in to unmask]
Subject: [TN] Flex Circuit


Dear Technetters


I am having coating adhesion problem with flex circuits. The cover plate
material is KAPTON or Poly imide. The conformal coating material used is
humiseal 2A64. The boards are cleaned, measuring less than 4 microgram Nacl
per sq in. against acceptable value of 10.6 max.

The flex circuit is dipped twice , followed by one spray. There is 15-20
bak between each dip. There is clear evidence of dewetting after first dip
and 2 dip. The spray coat is unacle to make all uniform - especially areas
which had dewetting. Fluoroscence is weak to Nil where dewetting occured.
That requires lengthly manual touch up work. Most of the dewetting is on
edges of the board.

We are interested in roughtening up the surface - Matt Finish in place of
Glossy Finish. We did scrubbed few samples and observed marked improvement
in adhesion of coating to surface.

Any one who can suggest IPC Standard, Military Standard or any other
industrial standard where this process step is specified as controlled
process ?

Our customer is Mil Standard, IPC and J-STD user and is concerned with
where Plasma etch is controlled process ?

Any help on this will be highly appreciated.

Regards

Ashok Dhawan
Solectron Winnipeg
(204) 631 7208

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2