Steve,
Well since I have spent 20 and half years working for essentially no-clean
companies (with one company for 9 months between Nortel and RIM that SHOULD
have cleaned!), others should probably have better suggestions than me on
how to clean them.
Bev
RIM
-----Original Message-----
From: Steven Kelly [mailto:[log in to unmask]]
Sent: Saturday, July 16, 2011 1:52 PM
To: [log in to unmask]; [log in to unmask]
Subject: Re: [TN] Ionic contamination problems
Thanks Bev,
According to both large connector manufacturers they do not do any testing
for cleanliness on their products before they ship.
So they are both incredibly bad as received and whether we can clean them up
remains to be seen.
Regards Steve
Steve Kelly
O (416) 750-8433
C (416) 577-8433
----- Original Message -----
From: Bev Christian [mailto:[log in to unmask]]
Sent: Friday, July 15, 2011 09:07 PM
To: 'TechNet E-Mail Forum' <[log in to unmask]>; Steven Kelly
Subject: RE: [TN] Ionic contamination problems
Steve,
I have found connectors to be among the dirtiest components. Part of that
may be all the nooks and crannies and another part may be that many
connector manufacturers are not as well funded as say a memory chip
manufacturer. Gather your evidence and get on the horn to your connector
supplier ASAP.
Bev
RIM
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steven Kelly
Sent: Friday, July 15, 2011 1:20 PM
To: [log in to unmask]
Subject: [TN] Ionic contamination problems
Hi All,
Today is my day for headaches.
We assembled a flex circuit (put a couple of connectors on) and did the
Ionic contamination test after our standard cleaning procedure and failed.
After much scratching of heads we decided to take a bare flex - solder it -
not add the connectors and test - passed the ionic test easily.
We then took the connectors and put them in the ionic unit - one hit 76
ug/cm2 as received and 6.9 after cleaning. The other was 9.6 ug/cm2 as
received and 6.6 after cleaning.
So my question is - do the connector manufacturers have to sign up for a
certain cleanliness level and second question what the *&?" do I do now.
Regards Steve Kelly
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|