Dave
I remember seeing a very similar problem on a low voltage ceramic hybrid a
few years ago but unfortunately it was a different company so I don't have a
lot of information but you may want to try:-
1. Cleaning the furnace muffle. If your muffle is as dirty as mine was it
could well be a source of sulfur.
2. Check to see if any of the operators smoke. The sulfur may be introduced
from their hands.
3. I seem to remember that we stopped using clear silicon gel (a 2 part Dow
Corning material) on these hybrids so it maybe worthwhile trying to build
and test a few circuits without encapsulant.
Hope this is some help
===== Original Message from TechNet@PAT [log in to unmask] (TechNet E-Mail
Forum.) at 24/09/98 02:08
>I need help tracing the possible root causes for a circuit failure from
>the field. Does anyone have any experience with open circuit traces due
>to a silver sulfide corrosion concentrated at the juncture tin-lead
>solder joints and silver thick films? We are seeing this only on joints
>that are low voltage potential. There is silver sulfide corrosion at
>other randomn areas, but the heavy corrosion is primarily at just a few
>points where the solder and silver meet. Under the microscope, it looks
>like a black worm crawling along the interface between the solder joint
>& the silver thick film. We pot the circuit board in silicone gel to
>protect the circuit from moisture. So far, we haven't traced the source
>of sulfur to any material that we use to make or to package the circuit
>board.
>The packaging does not contain cardboard, so sulfur from the packaging
>is out. We meticulously clean the board after reflow soldering the
>printed solder paste, so flux is out. Is it possible that we are getting
>sulfur gas from the enviroment? The environment is automotive,
>underhood. Is it possible that there is a galvanic action that is
>concentrating the corrosion to just a few solder joints?
>Thank you all for your time.
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
>To subscribe: SUBSCRIBE TechNet <your full name>
>To unsubscribe: SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional
information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
>################################################################
Mark Austin (Process Engineer)
ACW Technology Ltd
Hylton Road
Petersfield
GU32 3XX
TEL - (01730) 300000
FAX - (01730) 266045
DDI - (01730) 304401
MA @ ACW.CO.UK
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|