TECHNET Archives

October 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, David Suraski <[log in to unmask]>
Date:
Wed, 27 Oct 2004 08:41:44 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Jason Gregory <[log in to unmask]>
Subject:
From:
Jason Gregory <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (200 lines)
Paste was brand new and thoroughly warmed. Metal load on both pastes is
89.5% metal load.



Jason Gregory
Manufacturing Engineer
Innova Electronics
(281)653-5593
(281)653-5594 fax
(281)310-7588 cell
[log in to unmask]



-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of David Suraski
Sent: Wednesday, October 27, 2004 8:24 AM
To: [log in to unmask]
Subject: Re: [TN] Question about 2% Ag and stencil release


Daan's assessment sounds right. This could have been a paste dry out
issue.

Jason, do you know what the metal % was in each of these solder pastes?


Best regards,
David Suraski
AIM



-----Original Message-----
From: Jason Gregory [mailto:[log in to unmask]]
Sent: Wednesday, October 27, 2004 9:08 AM
To: [log in to unmask]
Subject: Re: [TN] Question about 2% Ag and stencil release

Yes, same flux in both pastes



Jason Gregory
Manufacturing Engineer
Innova Electronics
(281)653-5593
(281)653-5594 fax
(281)310-7588 cell
[log in to unmask]



-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Taheri, Kamran
Sent: Tuesday, October 26, 2004 7:39 PM
To: [log in to unmask]
Subject: Re: [TN] Question about 2% Ag and stencil release


Jason, did both solder pastes have the same flux chemistry?

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Daan Terstegge
Sent: Tuesday, October 26, 2004 4:00 PM
To: [log in to unmask]
Subject: Re: [TN] Question about 2% Ag and stencil release


Hi Jason,

I don't believe this has anything to do with silver.
The fine powder of your type 5 paste has a MUCH larger ratio between
soldersurface and soldervolume than the part 3 type, which means that it
is more difficult to keep the powder particles stable and oxide-free.
The smaller process window increases the chance of printing problems.
Hopefully a more accurate description will be given by one of the paste
manufacturers on this forum, but I think I'm pretty close....

Best regards,

Daan
http://www.smtinfo.net

----- Original Message -----
From: "Jason Gregory" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, October 26, 2004 9:44 PM
Subject: [TN] Question about 2% Ag and stencil release


> Has anybody had any experience or seen/written studies involving 2% Ag

> release from stencil apertures? We have a stencil, parts are small
resnets,
> about 15 mil pitch on a .006" thick stencil. Tried 2% silver paste
> (for tombstoning of other parts) with type 5 powder and had major
> release problems. We kept the same parameters on the screen printer
> (for reference/control purposes) and swapped in our "normal" 63/37
> Type 3
powder
> and release issues "virtually" went away. Not all the way, but for the
most
> part. I thought smaller mesh should have meant better release. Solder
> gurus ------- enlighten me!
>
> Jason Gregory
> Manufacturing Engineer
> Innova Electronics
> (281)653-5593
> (281)653-5594 fax
> (281)310-7588 cell
> [log in to unmask]
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
> unsubscribe, send a message to [log in to unmask] with following text in

> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
> -----------------------------------------------------
>
>

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2