Thanks for the input, Steve. These are being built using DuPont "LF"
material. Is that what you call "old-style?"




Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
      to Steve R Mikell <[log in to unmask]>



 To:      [log in to unmask]

 cc:      (bcc: Charles Barker/US/I-O INC)



 Subject: Re: [TN] Rigid-Flex Board baking









Charles Barker asked

*********************************************************************
Charles Barker
07/18/99 01:53 PM

To:   [log in to unmask]
cc:

Subject:  Board baking

We are just getting into regular assembly of rigid-flex boards. What are
folks doing about removing the moisture absorbed in the flex?

Is anyone using nitrogen as a drying agent?  What are sources of
"dry-boxes" and such?

All you flex makers out there, what do you recommend?

TIA

Charlie Barker

************************************************************************

Charlie,

Its a Monday, so give us some time to get cranked up.  First, are you
talking
old style or modern rigid-flex.
If you are using the old polyimide layers with acrylic adhesive, you can't
do
enough good things to guarantee success.
If, on the other hand, you are using the all polyimide construction, the
survivability is greatly enhanced.

If your boards are pre-baked and sealed in moisture proof bags, you may be
able to process without a prebake.  Moisture in your facility and time "out
of
bag" will determine the need and severity of your bake.  In cases like
these,
I always try and get any "scrappers" from the PWB fab house for
experiments.
2 hours at 105 C would be a good starting point if baking proves necessary.

Good luck,

Steve Mikell
Lead Ind. Eng.
Plant 13
SCI Systems

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################

ATOM RSS1 RSS2