Dan:
I have used the following stripping solution; water 16 parts, fluoboric
acid 2 parts, conc hydrogen peroxide(30%) 1 part. Immerse parts at room temp
with light agitation. Pay careful attention as the tin is stripped, do not
allow the reaction to proceed too far and attack the base metal. If they
have been sitting around too long after plate it may be difficult to strip
all the tin.
I would suggest that you use a copper barrier plate between the brass and
tin in the future. Good Luck!
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: Dan R. Johnson [mailto:[log in to unmask]]
Sent: Wednesday, September 25, 2002 11:51 AM
To: [log in to unmask]
Subject: [TN] stripping brass
Dear Technet,
Help!!!!
Can any of you metallurgical/chemical wizard types help me? I need to strip
tin (?) plate off of brass. Hopefully without etching the brass.
The plating solution was;
Flouboric Acid
Stannous Fluoroborate
Thiourea
This stuff soldered great last week but will not wet this week.
I greatly appreciate any help,
Dan
----------------------------------------------------------------------------
----- Technet Mail List provided as a free service by IPC using LISTSERV
1.8e To unsubscribe, send a message to [log in to unmask] with following text
in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/html/forum.htm for additional information, or
contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|