While in the AT&T facility at Richmond we had several complaints that due to
poor wetting of the surface finish the components were being sheared from
the board. When we investigated we found that the failure was not shear but
for the most part tensile. When we looked at the assembly operation we
always found that during assembly the boards were being bent and the failure
was in bending which explained why the stresses were for the most part
tensile. If you bend any board enough you will break the SMT joints. A pure
shear failure is much less likely to occur.
Best regards
Lee
J. Lee Parker, Ph.D.
JLP Consultants LLC
804 779 3389
----- Original Message -----
From: "Todd, Richard" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Thursday, January 11, 2007 6:03 PM
Subject: [TN] SMD Capacitor Shear Strength
> I have a question for the oracle . . .
>
> Does anyone know what is the solder joint shear strength for an 0603
> capacitor (assuming standard eutectic solder)?
>
>
>
> Regards,
>
>
>
> Rick Todd
>
> Senior Engineer
>
> Process Quality Engineering
>
>
>
> Panasonic Automotive Systems Company of America
>
> Division of Panasonic Corporation of North America
>
> 776 Highway 74 South, Peachtree City, GA 30269
>
> 770-515-1087 Direct
>
> 678-458-2887 Cell
>
> 770-486-2248 Fax
>
> [log in to unmask] <mailto:[log in to unmask]>
>
>
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|