The root cause is insufficient throwing power, but what caused that can
be traced back to a number of factors.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bush, Jeffrey D. (US
SSA)
Sent: Wednesday, September 09, 2009 1:17 PM
To: [log in to unmask]
Subject: Re: [TN] PTH problem
I would worry more about the units not failing test. Looks like no
current in plating - operator set the amps incorrectly - possibly this
is horizontal plating process - popular in Asia and is problematic in a
poorly controlled process environment.
Jeffrey Bush
Sr. Principle Product Assurance Engineer
Space Systems and Electronics - Performance Excellence
BAE SYSTEMS
P.O. Box 868, MER24-116A
Nashua, NH 03061-0868
Facility: 144 DW Highway
Merrimack, NH 03054
Office +1 603.885.8137
Mobile +1 603.318.8056
Fax +1 603.885.5258
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of J W
Sent: Wednesday, September 09, 2009 10:41 AM
To: [log in to unmask]
Subject: [TN] PTH problem
Hi TechNet group,
I'm really getting nervous about a China bare board supplier and their
quality and need your opinions. Please take a look at the picture by
clicking on the link below showing two plated through holes (via's).
The
problem reported originally was a bad ground connection between ground
via's
and ground planes. As you can see, the pictures are very telling, and
you
can clearly see the ground plane not connected (several planes not
connected
actually). What I'm also nervous about is the comment listed below the
pictures "The plated copper on PTH surface will be etched thin after OSP
process". Is that statement correct? I'm not a bare board expert by
any
means, but I believe a PTH should have a little more copper than what is
shown? I know that OSP is not something new, so are other board
suppliers
dealing with the same issue of possible thin PTH walls because of OSP?
I also submitted pictures early last week regarding the same supplier
having
problems with the their solder mask process, so to me, I'm thinking this
board shop is not up to standards and we should inform out board
assembler
house to look for another supplier...immediately?
Thanks for your help!
Jim
http://stevezeva.homestead.com/PTH_Connection_issue.jpg
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|