TECHNET Archives

June 2006

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
Dale Ritzen <[log in to unmask]>
Date:
Mon, 5 Jun 2006 11:04:23 -0500
MIME-Version:
1.0
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Dale Ritzen <[log in to unmask]>
Parts/Attachments:
text/plain (95 lines)
Quite a lot has been done in regard to this in the design of electronic
assemblies. There are some pretty good white papers out on part placement
changes during board design that minimize this risk, especially during
depanelization. I used to have one saved aside after an incident with a
customer of ours. I'll see if I can find it and post same.

The only solid way we were ever successful in finding these was with a quick
touch with a hot soldering iron. The cracked terminus usually pops off the
pad if it has cracked away from the body of the part. Yes, it does expose
the cap to another shot of high temp, but it does ensure that you detect all
cracked caps and get them replaced. Since caps with cracked terminus
typically don't fail consistently during ICT or functional testing (as they
can be in parallel or be making partial contact to pogo pins which still see
a device), the soldering iron method was our only recourse. But, this is
only practical if you have a consistent problematic area of the board. In a
case where the caps may be located in many areas, trying the soldering iron
technique on an entire board is probably not very timely or cost effective.

Good luck with this. It's a tough one...
Dale Ritzen
Quality Manager
Austin Manufacturing Services

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of John Maxwell
Sent: Monday, June 05, 2006 10:46 AM
To: [log in to unmask]
Subject: Re: [TN] Finding cracked capacitors


Daniel,
Most flex cracks are hidden under the termination at the capacitor
termination/PWA interrface making it very difficult to detect using SLAM
or C-SAM. A quick way to uncover cracks is exposure to humidity & bias
accelerating failure. A few temp cycles ahead of humidity testing will
open the cracks a bit easing humidity entering the capacitor body
accelerating failure.

John Maxwell


>A good acoustic microscope should be able to find these cracks quickly and
>non-destructively.  It is not a cheap tool, though, at $100k-$200k
depending
>on the options.
>
>On Mon, 5 Jun 2006 10:11:04 -0400, Tempea, Ioan <[log in to unmask]>
wrote:
>
>
>
>>Hi Technos,
>>
>>a never ending story, ceramic caps that crack, possibly due to
>>
>>
>depanelizing. The damage is not visible, unless the cap is cross sectioned.
>
>
>>Is there any testing, thermal cycling or something like that, that could
>>
>>
>show the damage real fast?
>
>
>>Thanks,
>>
>>Ioan
>>
>>

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2