TECHNET Archives

July 1999

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Transfer-Encoding:
7bit
Sender:
Subject:
From:
Andy Magee <[log in to unmask]>
Date:
Sat, 24 Jul 1999 08:08:02 -0400
Content-Type:
text/plain; charset=us-ascii
MIME-Version:
1.0
Reply-To:
Parts/Attachments:
text/plain (62 lines)
Sulfuric is preferred over Hydrochloric for oxide removal because HCl
tends to increase in etch activity as the dissolved copper concentration
goes up with use. 10% H2SO4 will be a much more stable and reliable
process for oxide removal. Save the nitric for things like stripping
copper off your plating racks.

Andy Magee
Flex Guru - Consulting
[log in to unmask]
(937) 435-3629

ps. Initially copper foil is provided from the supplier with a zinc
chromate passivation coating to prevent oxidation. Since this angstroms
thick, relatively brittle, layer may not be uniformly intact it should
be removed with a process that will not attack the copper before
microetching. 10% H2SO4 is clearly the preferred choice over HCl, but
there are also a number of proprietary acid/surfactant mixtures that are
widely used for this.


LeRoy wrote,

Subject: Re: Copper oxide removal
Date: Fri, 23 Jul 1999 15:56:52 -0400
From: LeRoy Forney <[log in to unmask]>

My understanding of the usual oxide removal procedure is a 3-minute soak
with 5%HCl.  The goal is a very mild
etch, and I've heard that nitric acid will cause pitting instead - and
this is in line with some laboratory
oxidation studies I did some time ago.  Variability in solderability
data was much higher on aged coupons I had
treated with dilute HNO3 than on coupons treated with 5%HCl.

LeRoy
-----Original Message-----
From:   nishath yasmeen [SMTP:[log in to unmask]]
Sent:   Friday, July 23, 1999 3:34 PM
To:     [log in to unmask]
Subject:        [TN] Copper oxide removal

Hello everyone!
    Is Nitirc acid ( dilute)  a better acid than sulfuric for cleaning
the oxide on plated copper?
    Any information provided will be appreciated.

Yasmeen

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################

ATOM RSS1 RSS2