Hi Paul - And you thought solderability was a simple subject! The
solderability comparison data you were looking at was developed using a
wetting balance. During the wetting balance test the fluxed test sample is
lowered into the solder pot (or some equipment uses a solder globule). As
solder "wets" the surface in the case of a tin/lead finish or the finish
diffuses in the case of gold (silver, etc.) an force measurement device in
the wetting balance test head records the force values - basically Young's
equation. The buoyancy of the test sample (the amount of molten solder the
test sample bulk displaces) as it enters the solder bath does give the
instrumentation a negative force but that can be calculated out of the
measurement leaving you with a the wetting force. If a test sample is not
solderable the end result would be a negative force as describe in the
paper you read - no wetting occurred thus no force pulling down on the
specimen to be recorded. An analogy would be dipping your finger coated
with oil into soapy water - you wouldn't get the water to wet your finger
until the soap dissolves the oil allowing the water to wet up your finger
creating a positive wetting force. Take a look at chapter 7.2.1 Wetting
Balance Method in Klein Wassink's book (ISBN 0-901150-14-2) for a better
description and more information. In the gold case you mention if once the
gold diffuses into the solder pot and the underlying substrate is not
wettable then a negative force would result. Hope this helps.
Dave Hillman
Rockwell Collins
[log in to unmask]
PAUL BROWN <[log in to unmask]> on 06/15/99 02:42:17 PM
Please respond to [log in to unmask]
To: [log in to unmask]
cc:
Subject: [TN] negative force
Hi all,
I was just reading a paper which was comparing the solderability of
different surface finishes. In it the show electroless nickel/ immersion
gold to have a wetting force of 0 uN/mm at "2 sec" just after
fabrication. this value becomes negative i.e -0.1 to -0.2 after reflow
ect.... What does this mean? Does this mean that solder is actually
repelled by Ni/Au finish? Is this only due to the short duration
(2sec.) that the dip occurred? Does the value become positive; at say 5
seconds ? How does this affect a surface mount assembly, will parts be
displaced prior to soldering? I was under the impression that gold was
highly solderable......................I need help, but will settle for
answers...............Paul Brown
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section
for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|