Good Morning Dan! From an assembly point of view your temperatures are
pretty workable for a reflow profile but the ramp rates are somewhat
restrictive. I have seen multiple instances of reflow processes running at
ramp up/down rates of 4-6 C/sec with no danger of impacting the component
integrity. Is there a material rationale for the 2 C/sec ramp rate
suggestion? As an assembler I am always give preference to components with
the maximum reflow profile robustness.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Dan R. Johnson" <[log in to unmask]>@ipc.org> on 02/20/2002 03:14:49 PM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
to "Dan R. Johnson" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
To: [log in to unmask]
cc:
Subject: [TN] Safe processing window
A couple of questions for what has become my best engineering resource.
Management has asked me to provide a re-flow profile for our product, a
surface mount component built on FR-4 with lead free solder. I am
reluctant, I would prefer to generate a "safe processing window" type
document. As manufacturing professionals what do you prefer?
The window would spec ; max 2 C /sec ramp up, max 60 sec dwell above 180
C, max 220 C peak, and a 2 C/sec max ramp down. Could you live with this?
Many thanks for your help,
Dan
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|