TECHNET Archives

February 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Date:
Fri, 27 Feb 2009 18:13:20 +0000
Reply-To:
Subject:
From:
Vladimir Igoshev <[log in to unmask]>
MIME-Version:
1.0
In-Reply-To:
Content-Type:
text/plain
Content-Transfer-Encoding:
base64
Parts/Attachments:
text/plain (1 lines)
Thank you Richard for expanding my short replies :-)



Vladimir

SENTEC

11 Canadian Road, Unit 7.

Scarborough, ON M1R 5G1

Tel: (416) 899-1882

Fax: (905) 882-8812

www.sentec.ca





-----Original Message-----

From: "Stadem, Richard D." <[log in to unmask]>



Date:         Fri, 27 Feb 2009 11:11:56 

To: <[log in to unmask]>

Subject: Re: [TN] Reflowing CBGA component (with high Sn balls) using Eutectic solder paste





Just to clear up the confusion from the previous responses:



To my knowledge, the IBM PowerPC components are ceramic ball joint

arrays (CBGAs) that utilize a Pb90 ball, not Sn90. The melting

temperature of these primarily lead balls is way up over 250 deg. C.

They are not intended to be brought into liquidus. These lead balls are

attached to the CBGA package with Sn63 solder, and they are intended to

be used with standard Sn63 solder paste to form the SJ to the pads on

the assembly. 



Ceramic-body CBGAs typically use Pb90 solder balls because the lead

balls have a higher modulus of elasticity, providing some strain relief

between the very low CTE of the alumina oxide component and the higher

CTE of a standard FR-4 PWB.

 

Because the Pb90 BGA balls do not go into liquidus, but the Sn63 paste

does, a small amount of the lead ball dissolves into the molten Sn63 to

form the solder joint.

It is important, however, to either increase the standard reflow profile

and/or the MRT slightly to get good wetting of the Sn63 solder over the

Pb90 ball and get a good homogenous mix, but you do NOT need to melt the

Pb90 ball. 

I have found that if you attempt to use the standard reflow profile you

will get what Mr. Macko is seeing, good wetting on the board pad, but

not quite perfect on the Pb90 ball. Increasing the TALT or the MRT

slightly (perhaps by 10 deg. C) usually fixes the issue.



If your IBM PPC CBGAs do in fact have Sn90Pb10 solder balls, then you

would use a Pb-free profile with enough TALT and a high enough MRT to

form a good homogenous SJ.



I do not have any experience with soldering Pb90 CBGAs with lead-free

solder, but I assume the principle is the same as soldering with Sn63.

However, with the higher temperature lead-free profile and using a Sn99

solder, I am assuming more of the lead ball will be dissolved into the

solder joint, and the homogenity will be less, which will result

possibly in a solder joint of lesser reliability. But I may be wrong

about that. Others with experience in this care to comment?



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Joe Macko

Sent: Friday, February 27, 2009 10:04 AM

To: [log in to unmask]

Subject: [TN] Reflowing CBGA component (with high Sn balls) using

Eutectic solder paste



Hi All,



 



My question is related to the soldering of IBM PPC CBGAs type components

(that have Sn90Pb10 solder balls) using Sn63 paste onto ENIG finished

boards.  What are the "determining-factors" to improve the

wetting/diffusion of the eutectic solder paste into the high Sn solder

balls. The eutectic solder appears to wet well to the ENIG pads located

on the board but occasionally I see eutectic solder fillets that do not

always appear to fuse well with the high Sn content balls (if fuse is

the correct word?).  thx



 



 



Best Regards,



-Joe



 





"This e-mail and any attachments are solely for the use of the addressee

and may contain L-3 proprietary information that may also be defined as

U.S. Government export controlled technical data. If you are an

unintended recipient of this e-mail, use, disclosure or distribution of

its content is prohibited. Please notify the sender by return e-mail and

immediately delete this message."

 





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To

unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or

(re-start) delivery of Technet send e-mail to [log in to unmask]: SET

Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the

posts: send e-mail to [log in to unmask]: SET Technet Digest Search the

archives of previous posts at: http://listserv.ipc.org/archives Please

visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for

additional information, or contact Keach Sasamori at [log in to unmask] or

847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------




ATOM RSS1 RSS2