TECHNET Archives

November 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Fri, 5 Nov 2004 08:20:08 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Content-type:
text/plain; charset="us-ascii"
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
In-Reply-To:
MIME-Version:
1.0
Parts/Attachments:
text/plain (141 lines)
Hi Ken! Now those are interesting photos! The "typical black pad" defect
associated with ENIG surface finishes is more subtle than what is
illustrated in your photos. My guess is that you are dealing with a severe
breakdown of the plating process on those affected pads - the amount/type
of disturbance of the pad finish is extreme. It almost appears that you had
some organic contamination of those pads which is reacting with the
solderpaste deposit. Let us know what the microsections reveal.

Dave Hillman
Rockwell Collins
[log in to unmask]




             Ken Patel
             <[log in to unmask]
             OM>                                                        To
             Sent by: TechNet          [log in to unmask]
             <[log in to unmask]>                                          cc

                                                                   Subject
             11/04/2004 12:29          Re: [TN] Solderability issue...
             PM


             Please respond to
              TechNet E-Mail
                   Forum
             <[log in to unmask]>
             ; Please respond
                    to
                 Ken Patel
             <[log in to unmask]
                    OM>






Steve and all,
Our CM is using no clean AIM solder paste and we think that there is no
problem from that angle. When I personally went and looked the board, the
quality person told me that she is seeing black color on the pad. I laughed
at saying that can't happen on my boards after problem was fixed in the
industry 5-7 years ago and what you are seeing must be reflection (optical
illusion) of black molded QFP or similar components on a very shinny solder
joint. And also ALL fab house knows the black pad phenomenon and they
control the phosphorous content in nickel bath to prevent this from
happening!

I looked board from different angles, took to different microscopes and
also
used couple of regular magnifying glasses to clear any doubts about the
blackish looking pads. And indeed it turned out black/dark gray. We found
some locations were you can see thru naked eye. What surprised me was only
passives were affected, mostly on one side of the board. Also one pad was
affected 1/2 making solder joint half as there was de-wetting on the black
part portion.

Few equations for TechNet experts:
        (1) Why only one side was affected more than other?
        (2) Why only few locations are affected and not the entire board?
        (3) Why problem persists more near the edge of the board then the
center of the board?
        (4) Why name black pad was given - is it due to black color looking
pads?
        (4) Can this be reworked?

We have given board for cross section to confirm the problem. I will update
you with the finding.

Re,
Ken Patel


Hi Ken and TechNetters!

Ken sent me some pictures of some solder problems he's seeing on some
assemblies and wanted me to post them on my page. I got the pictures up. Go
look at:

http://www.stevezeva.homestead.com/files/solderability_1.jpg

http://www.stevezeva.homestead.com/files/solderability_2.jpg

http://www.stevezeva.homestead.com/files/solderability_3.jpg

I have a few questions; are you seeing this quite a bit, or just very
random? What kind of solder paste is it?

I had some strange looking joints one time in the past when I was out in
California building memory modules. We were using water soluble paste at
the
time. One of the inspectors called me said that she was seeing cold solder.
I went and looked at the assembly, and saw what really did look like cold
solder. But the strange thing was that it was occuring on a couple of leads
on a part, and all the rest of the leads were fine...including the ones
right next to the leads that looked cold.

I was thinking;"Something doesn't add up, convection heat doesn't work like
this...how can one lead have cold solder, then the one right next to it is
fine?"

I started looking a little more, and took a pair of tweezers and gently
probed the cold solder joint. To my suprize, there was a solid fillet of
solder that was wetted to the lead and pad beneath a layer of what looked
like cold solder. Things were getting really strange now.

To make a long story short, what it turned out to be was that the screen
print operator was using a wet rag to clean the underside of the stencil
periodically. It was an old MPM SP2400 that didn't have an automatic
cleaning system. The operators heart was in the right place, but the rag he
was using was overly wet. When he wiped the bottom of the stencil, some of
the water was trapped in the apertures. So on the next print, the was
enough
water to alter the chemistry of the past that gave us these random cold
looking solder joints.

After I took his wet rag away, gave him some decent wipes and alcohol, the
problem went away.

The point of this story is that maybe whatever they're using to clean the
stencil with might becoming trapped in some of the apertures, and the
screwing the paste up on the next couple of prints.

Just a WAG...

-Steve Gregory-

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2