Your failure mode of deepest concern is most likely CAF (Conductive
Anodic Filament). The most common spot for this problem is via to
trace, and the seed is disturbances in the via side wall. CAF can also
grow along glass filaments within pre-preg from layer to layer. Failure
potentials are at less than 10% of the 750V/mil. Laminates are
available with very high CAF resistance if you need to push things. I
believe there are some BT based materials that are virtually immune, but
1500V is a lot of potential!
Wayne Thayer
>>> [log in to unmask] 9/25/2006 5:06 pm >>>
Should I be using IPC Table 6.1 for conductor spacing for high voltage
in the z-axis of the pcb?
Or should I be using the approximately 750V/mil spec from the laminate
supplier and derate that number?
Board has +/- 1200V.
Thank you.
Kaye Clayo
Sr. P. C. Layout Designer
Keithley Instruments, Inc.
440-498-2862
CONFIDENTIALITY NOTE: This message is intended only for the use of the
individual or entity to which it is addressed and may contain
information that is privileged, confidential, and exempt from disclosure
under applicable law. If the reader of this notice is not the intended
recipient, you are hereby notified that any dissemination, distribution
or copying of this communication is strictly prohibited. If you have
received this communication in error, please notify the sender
immediately.
_____________________________________________________________________________
Scanned by IBM Email Security Management Services powered by
MessageLabs. For more information please visit http://www.ers.ibm.com
_____________________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|